The tendencies of advancement of nickel-based superalloys for casting turbine blades of aircraft engines are considered. Using the method of mathematical planning of the experiment, quantitative regularities of the influence of alloying elements W, Mo, Cr, Co, Ti, Nb, Hf and C on the durability at 975 °C and stress 200 MPa of castable polycrystalline nickel-based superalloys of the VZhL12U type with low density were established. Concentration regression models of the durability of alloys of this type are developed. It was found that the alloying elements W and Mo in the studied concentration range have a positive effect on the durability of alloys of the VZhL12U type. With an increase in the content of Ti, Nb, and C within the studied concentration range, the durability of alloys decreases, an increase in the Hf content leads to an increase in the durability of alloys of this type. The positive effect of W on durability decreases with an increased Cr content in the alloy. When the Cr content in the alloy is more than 8 wt. % the durability is decreases.
The effect of Co on the durability of VZhL12U alloys is ambiguous. Alloys show the minimum values of durability with a Co content equal to 11–12 wt. % At lower or higher concentrations of Co, the durability of the alloys increases.
It is shown that a decrease in the durability of alloys of the VZhL12U type with an increase in the content of Ti and Nb is associated with the formation of a significant amount of the γ+γ' eutectic.
It has been established that the alloying of VZhL12U alloys with hafnium increases the γ'-solvus temperature Tsolv to 1258 °С, decreases the solidus temperature TS to 1260 °С and the temperature of the onset of crystallization Tcr to 1320 °С, and doe
2. Gabb T.P., Dreshfill R.L. Properties of superalloys. Superalloys II. Heat-resistant materials for aerospace and industrial power plants: in 2 books Moscow: Metallurgy, 1995, book 2, pp. 352–371.
3. Logunov A.V. High-temperature nickel alloys for gas turbine blades and discs. Rybinsk: Gazoturbinnyye tekhnologii, 2017, 854 p.
4. Kablov E.N., Golubovsky E.R. Heat resistance of nickel alloys. Moscow: Mashinostroenie, 1998, 464 p.
5. Donachie M.J., Donachie S.J. Selection of superalloys for design. Mechanical Engineeres Handbook. 3rd ed. John Wiley & Sons. Inc, 2006. vol. 1. pp. 287−334.
6. Kishkin S.T., Polyak E.V. Kinetics of fracture of high-temperature alloys during creep. Creation, research and application of heat-resistant alloys: selected works. Moscow: Nauka, 2006, pp. 92–105.
7. Stepanov V.M., Kishkin S.T., Chumakov V.A., Chubarov V.G., Demonis I.M. Progressive methods of precision casting of GTE blades. Creation, research and application of heat-resistant alloys: selected works. Moscow: Nauka, 2006. pp. 304–310.
8. Cast blades of gas turbine engines. Alloys, technologies, coatings. Ed. E.N. Kablov. 2nd ed. Moscow: Nauka, 2006, 632 p.
9. Kablov E.N., Echin A.B., Bondarenko Yu.A. History of development of directional crys-tallization technology and equipment for casting blades of gas turbine engines. Trudy VIAM, 2020, no. 3 (87), paper no. 01. Available at: http://www.viam-works.ru (accessed: November 6, 2020). DOI: 10.18577/2307-6046-2020-0-3-3-12.
10. Kishkin S.T., Sobolev G.I., Stepanov V.M. et al. Heat-resistant alloy ZhS6-F-NK. Creation, research and application of heat-resistant alloys: selected works. Moscow: Nauka, 2006, pp. 277–281.
11. Ross I.V., Sims Ch.T. Nickel-based alloys. Superalloys II. Heat-resistant materials for aerospace and industrial power plants: in 2 books. Moscow: Metallurgiya, 1995, book. 1, pp. 128–174.
12. Glenny R. J., Northwood J. E., Burwood-Smith A. Materials for gas turbines. International Metallurgical Reviews, 1975, vol. 20, pp. 1–28.
13. Quested P.N., Osgerby S. Mechanical properties of conventionally cast, directionally solidified, and single-crystal superalloys. Materials Science and Technology, 1986, vol. 2, pp. 461–475.
14. Shalin R.E., Svetlov I.L., Kachanov E.B., Toloraya V.N., Gavrilin O.S. Single crystals of nickel heat-resistant alloys. Moscow: Mashinostroenie, 1997, 336 p.
15. Kablov E.N., Toloraia V.N., Orekhov N.G. Monocrystalline nickel rhenium-containing alloys for turbine blades of gas turbine engines. Metallovedenie i termicheskaya obrabotka metallov, 2002, no. 7, pp. 7-11.
16. Gerasimov V.V. From single-crystal uncooled blades to turbines blades with penetration (transpiration) cooling made by additive technologies (review on technology of single-crystal GTE bladescasting). Trudy VIAM, 2016, no. 10, paper no. 1. Available at: http://www.viam-works.ru (accessed: November 6, 2020). DOI: 10.18577/2307-6046-2016-0-10-1-1.
17. Casting alloy based on nickel: pat. RU 722330 C; filed 29.12.78; publ. 30.11.94.
18. Nickel-based alloy: pat. RU 1412342 C; filed 02.12.86; publ. 30.11.94.
19. Kablov E.N., Svetlov I.L., Petrushin N.V. Nickel high-temperature alloys for casting blades with directional and monocrystalline structure. Part 1. Materialovedenie, 1997, no. 4, pp. 32–39.
20. Hoppin J.S., Deinesi W.P. The future of superalloys. Superalloys II. Heat-resistant materials for aerospace and industrial power plants: in 2 books. Moscow: Metallurgiya, 1995, book 2, pp. 325–344.
21. Erickson G.L., Harris K. DS and SX superalloys for industrial gas turbines. Proceedings of a Conference held in Liège. Kluwer Academic Publishers, 1994, part II: Materials for Advanced Power Engineering, pp. 1055–1074.
22. Erickson G.L. A new third generation single crystal casting superalloys. Journal of Metals, 1995, vol. 47, no. 4, pp. 36–39.
23. Walston S., Cetel A., MacKay R. et al. Joint development of a fourth generation single crystal superalloy. Superalloys 2004. Minerals, Metals & Materials Society, 2004, pp. 15–24.
24. Koizumi Y., Kobayashi T., Yokokawa T. et al. Development of next-generation Ni-base single crystal superalloys. Superalloys 2004. Minerals, Metals & Materials Society, 2004, pp. 35–43.
25. Shein E.A. Tendencies in the field of alloying and microalloying of heat resisting single-crystal alloys on the basis of nickel (review). Trudy VIAM, 2016, no. 3, paper no. 02. Available at: http://viam-works.ru (accessed: November 10, 2020). DOI: 10.18557/2307-6046-2016-0-3-2-2.
26. Petrushin N.V., Ospennikova O.G., Svetlov I.L. Single-crystal Ni-based superalloys for turbine blades of advanced gas turbine engines. Aviacionnye materialy i tehnologii, 2017, no. S, pp. 72−103. DOI: 10.18577/2071-9140-2017-0-S-72-103.
27. Wahl J.B., Harris K. New single crystal superalloys, CMSX-7 and CMSX-8. Superalloys 2012. Minerals, Metals & Materials Society, 2012, pp. 179−188.
28. Li J.R., Liu S.Z., Wang X.G. et al. Development of a low-cost third generation single crystal superalloy DD9. Superalloys 2016. Minerals, Metals & Materials Society, 2016, pp. 57−63.
29. Ospennikova O.G. Tendencies of development of heat-resistant nickel alloys of low density with polycrystalline and single-crystal structures (review). Aviacionnye materialy i tehnologii, 2016, no. 1 (40), pp. 3–19. DOI: 10.18577/2071-9140-2016-0-1-3-19
30. Nickel-based heat-resistant alloy for monocrystalline casting: pat. RU 2439184 C1; filed 05.10.10; publ. 10.01.12.
31. Petrushin N.V., Ospennikova O.G., Visik E.M., Rassokhina L.I., Timofeeva O.B. Low-density heat-resistant nickel alloys. Liteinoe proizvodstvo, 2012, no. 6, pp. 5−11.
32. Kablov E.N., Ospennikova O.G., Petrushin N.V., Visik E.M. Single-crystal nickel-based superalloy of a new generation with low-density. Aviacionnye materialy i tehnologii, 2015, no. 2 (35), pp. 14–25. DOI: 10.18577/2071-9140-2015-0-2-14-25.
33. Nickel Basislegierung für die gießtechnische Herstellung einkristallin erstarrter Bauteile: pat. DE 10100790 C2; filed 15.12.01; publ. 18.07.02.
34. Low density, high creep resistant single crystal superalloy for turbine airfoils: pat. US 7261783; filed 22.09.04; publ. 28.08.07.
35. Kablov E.N., Toloraya V.N., Ostroukhova G.A. Growth structure of monocrystalline castings from nickel heat-resistant alloys. Foundry heat-resistant alloys. The effect of S.T. Kishkina. Moscow: Nauka, 2006, pp. 219–245.
36. Ross E.W., O'Hara K.S. RENE N4: A first generation single crystal turbine airfoil with improved oxidation resistance, low angle boundary strength and superior long time rupture strength. Superalloys 1996. Minerals, Metals & Materials Society, 1996, pp. 19–25.
37. Kuleshova E.A., Glezer G.M., Petrushin N.V. Influence of structure parameters on the service characteristics of casting high-heat-resistant nickel alloys. Proceedings of the Internet. Scientific and Technical Conf. “Scientific ideas of S.T. Kishkina and modern materials science”. Moscow: VIAM, 2006, pp. 200–211.
38. Kablov E.N. Innovative developments of FSUE «VIAM» SSC of RF on realization of «Strategic directions of the development of materials and technologies of their processing for the period until 2030». Aviacionnye materialy i tehnologii, 2015, no. 1 (34), pp. 3–33. DOI: 10.18577/2071-9140-2015-0-1-3-33.
39. Lukovkin A.I., Pankratov V.A., Petrushin N.V. et al. Influence of zirconium and hafnium on long-term strength and crack resistance of nickel alloys with an increased tungsten content. Aviatsionnaya promyshlennost, 1984, no. 12, pp. 53–56.
40. Dolzhansky Yu.M., Stroganov G.B., Shalin R.E. Optimization of the properties of engineering materials using a computer. Moscow: Publishing house of the USSR Ministry of Defense, 1980, 395 p.
41. Petrushin N.V., Ignatova I.A., Logunov A.V. et al. Investigation of the dimensional mismatch between the periods of the crystal lattices of the γ- and γʹ-phases on the characteristics of the heat resistance of precipitation-hardening nickel alloys. Izvestiya AN SSSR, ser.: Metals, 1981, no. 6, pp. 153–159.
42. Lashko N.F., Zaslavskaya L.V., Kozlova M.N. et al. Physicochemical phase analysis of steels and alloys. Moscow: Metallurgiya, 1978, 336 p.
43. Petrushin N.V., Logunov A.V., Kishkin S.T. et al. Investigation of the regularities of changes in physical and mechanical properties and structural stability of nickel heat-resistant alloys. Aviation materials. Moscow: VIAM, 1983, is: Thermophysical studies of heat-resistant alloys and heat-shielding coatings, pp. 17–30.
44. Morozova G.I. Physicochemical phase analysis in the study of heat-resistant nickel alloys. Proceedings of the Internet. Scientific and Technical Conf. “Scientific ideas of S.T. Kishkina and modern materials science”. Moscow: VIAM, 2006, pp. 160–168.
45. Bokshtein S.Z., Ignatova I.A., Bolberova E.V., Kishkin S.T., Razumovsky I.M. Influence of mismatch of lattice parameters of phases on the diffusion permeability of interphase boundaries. Fizika metallov i metallovedeniye, 1985, vol. 59, is. 5, pp. 936–942.
The trends in the development of technologies for the manufacture of metal products presented in the article determine future directions in the production of products of maximum complexity. Over the past 30 years, new technologies for the manufacture of precision parts using metal powders have gained significant weight in many technical industries: electronics, machine tools, aerospace, medicine, and motor transport. In the case of manufacturing parts of complex geometric shapes, small dimensions and mass, foreign companies have introduced technologies for injection molding of metal-powder compositions – Metal injection molding or MIM technology. In comparison with the existing technologies of casting and powder metallurgy, MIM technology provides several times reduction in the cost of manufacturing parts of complex geometric shapes. The prospects and competitiveness of MIM technologies are determined by such advantages as: the ability to manufacture parts of complex shapes; no additional operations (for example, machining) to obtain a finished part and, as a result, a high material utilization rate – from 96 to 99%; the ability to manufacture parts with a minimum wall section thickness of 0.5 mm; high productivity of the process and the possibility of full automation of production.
In the manufacture of parts using the MIM technology, compact technological equipment is used; there is no need for a melting section in production. The main prerequisites for the development of MIM technology in modern machine building were the expansion of the range of powders and binders, equipment for controlling their quality, methods for obtaining powders of spherical shape and controlled size, as well as equipment for producing mixtures of powders with a binder. The use of such technologies made it possible to obtain high-quality raw materials for MIM technology &
2. Chainov N.D., Myagkov L.L., Moskvichev Yu.P. New structural materials – granular composites and the effectiveness of their application in engine building. Collection of scientific. tr. Int. conf. "Engine-2010", dedicated to 180th anniversary of N.E. Bauman MSTU. Moscow, 2010, pp. 67–70.
3. Tverskoy M.V., Khilkova A.A., Khilkov D.E. Investigation of the features of injection molding of metal powder mixtures. Politekhnicheskiy molodezhny zhurnal N.E. Baumana MGTU, 2018, no. 11 (28), pp. 406–407.
4. Ramakrishnan P. Automotive applications of powder metallurgy. Advances in powder metallurgy, 2013, no. 7, pp. 493–519.
5. Semenov B.I., Semenov A.B., Muranov A.N. Processing and properties of superalloys suitable for MIM. Modern heat-resistant wrought nickel and intermetallic alloys, methods of their processing: collection of articles of conf. Moscow: VIAM, 2015, pp. 10–13.
6. Hausnerova B. Powder Injection Molding as an Alternative Processing Method for Automotive Items. PIM International, 2011, no. 3, pp. 129–146.
7. Semenov A.B., Muranov A.N., Kutsbakh A.A., Semenov B.I. Injection molding of structured multiphase materials. Vestnik RUDN, ser.: Engineering research, 2017, vol. 18, no.4, pp. 407–425.
8. Semenov A.B., Muranov A.N., Semenov B.I. Thixo- and PIM-technologies in modern engine building. Gruzovik, 2017, no. 10, pp. 3–6.
9. Public analytical report in the direction of "New production technologies". Moscow: Skolkovo Institute of Science and Technology, 2015, 210 p.
10. Pogodina E. Casting of powder mixtures. Plastiks. Effektivnye TPA, 2013, no. 6 (124), pp. 34–36.
11. Parkhomenko A.V. Development of binders in granulates for MIM technology. Vestnik Samarskogo gosudarstvennogo tekhnicheskogo universiteta, ser.: Technical sciences. 2013, no. 2, pp. 91–98.
12. Starting material for injection molding of metal powder: pat. US 5006164A; filed 02.26.90; publ. 09.04.91.
13. Peskova A.V., Sukhov D.I., Mazalov P.B. Exami-nation of the formation of the titanium alloy VT6 structure obtained by additive manufacturing. Aviacionnye materialy i tehnologii, 2020, no. 1 (58), pp. 38–44. DOI: 10.18577 / 2071-9140-2020-0-1-38-44.
14. Korotchenko A.Yu., Kotomin S.V., Tverskoy M.V., Khilkov D.E. Development of a new composition of a metal powder mixture for molding under pressure. Liteynoye proizvodstvo, 2018, no. 2, pp. 23–27.
15. Muranov A.N. Investigation of free shrinkage of the main types of polymer-powder mixtures used for the manufacture of parts from powder analogs of 38KhMA (42CrMo4) steel by the MIM method. Mekhanika kompozitsionnykh materialov i konstruktsiy, 2019, vol. 25, no. 1, pp. 76–86.
16. Yakovlev A.L., Arislanov A.A., Putyrsky S.V., Nochovnaya N.A. Study of mechanical properties and structure of large-sized semi-finished products made of VT6ch titanium alloy. Aviacionnye materialy i tehnologii, 2020, no. 4 (61), pp. 12–18. DOI: 10.18577 / 2071-9140-2020-0-4-12-18.
17. Parkhomenko A.V. Characteristics of MIM granules based on carbonyl iron powder of the NM grade and polyformaldehyde. Intellektualnyj potentsial XXI veka: stupeni poznaniya, 2016, no. 32, pp. 89–93.
18. Thermoplastic masses for preparing metallic moldings: pat. EP 0465940-B1; filed 15.01.92; publ. 17.05.95.
19. Semenov A.B. Development of a methodology for mathematical modeling of the process of injection molding of polymers filled with metal powders. Tekhnologiya metallov, 2019, no. 1, pp. 9-16.
20. Semenov A.B., Semenov B.I. Two paradigms of metal casting technologies. Izvestiya vuzov. Mechanical engineering, 2017, no. 5, pp. 79–98.
21. Kablov E.N., Evgenov A.G., Ospennikova O.G. et al. Metal-powder compositions of EP648 heat-resistant alloy produced by FSUE "VIAM" State Scientific Center of the Russian Federation in technologies of selective laser alloying, laser gas-powder surfacing and high-precision casting of polymers filled with metal powders. Izvestiya vuzov. Mechanical engineering, 2016, no. 9, pp. 62–80.
22. Froes (Sam) F.H. Advances in titanium metal injection molding. Powder Metallurgy and Metal Ceramics, 2007, vol. 46, p. 303–310.
23. German R.M. Powder Metallurgy Science. 2nd ed. New Jersey: MPIF Princeton, 1994. Chap. 6. 192 p.
24. Froes (Sam) F.H., Yau Te-Lin, Weidenger H.G. Titanium, Zirconium and Hafnium. Chap. 8. Materials Science and Technology – Structure and Properties of Nonferrous Alloys. Ed. K.H. Matucha. Weinheim: VCH, 1996, p. 401.
25. Froes (Sam) F.H. Titanium. Encyclopedia of Materials Science and Engineering. Oxford: Elsevier, 2000, pp. 328–340.
26. Froes (Sam) F.H. Titanium Alloys. Handbook of Advanced Materials. Wessel: Wiley Interscience, 2004. P. 271.
27. Froes (Sam) F.H. Titanium Metal Alloys: Handbook of Chemical Industry Economics, Inorganic. New York: John Wiley and Sons Inc., 2000, pp. 44–50.
28. Kang L. Ceramic Membranes for Separation and Reaction. London: John Wiley and Sons, 2007, 306 p.
29. Boljanovic V. Powder metallurgy. Metal Shaping Processes: Casting and Molding, Particulate Processing, Deformation Processes, Metal Removal. New York: Industrial Press Inc., 2009, pp. 325–346.
30. Gülsah E., Bülent A., Özkan Gülsoy H. Injection molding of micro-porous titanium alloy with space holder technique. Rare Metals, 2011, no. 30, pp. 565–571.
31. Yakovlev A.L., Nochovnaya N.A., Putyrskij S.V., Krohina V.A. Titanium-polymer laminated materials. Aviacionnye materialy i tehnologii, 2016, no. S2, pp. 56–62. DOI: 10.18577/2071-9140-2016-0-S2-56-62.
32. Korotchenko A.Yu., Kovalevich E.V., Nuraliev N.F., Kutsy O.Ya. A device for the study of free casting shrinkage of alloys. Liteinoe proizvodstvo, 2020, no. 11, pp. 16–18.
33. Korotchenko A.Yu., Khilkov D.E., Tverskoy M.V., Khilkova A.A. On the use of additive and hybrid technologies in foundry. Liteinoe proizvodstvo, 2019, no. 6, pp. 26–28.
34. Kablov E.N., Kashapov O.S., Medvedev P.N., Pavlova T.V. Study of a α+β-titanium alloy based on a system of Ti–Al–Sn–Zr–Si–β-stabilizing alloying elements. Aviacionnye materialy i tehnologii, 2020, no. 1 (58), pp. 30–37. DOI: 10.18577/2071-9140-2020-0-1-30-37.
35. Kablov E.N. The dominant feature of the national technology initiative. Problems of accelerating the development of additive technologies in Russia. Metally Evrazii, 2017, no. 3, pp. 2–6.
Various alloys belonging to the Ti–Al system have been studied in the area of intermetallic phases existence. Phase diagrams of the Ti–Al system are presented. The main ordered compounds of this system are shown: the γ-TiAl phase, the Al2Ti phase (in the form of the h-and r-phases), the metastable Al5Ti3 phase, and the Al3Ti phase, the two latter possessing single- and long-period superstructures.
Among the intermetallic compounds of the Ti–Al system gamma alloys based on the γ-TiAl phase are currently the most studied and have found practical applications. As a result of the accomplished analysis of scientific and technical sources there has been identified an area in the Ti–Al system containing potentially promising titanium aluminides which possess lower density and higher Young’s modulus compared to those of gamma alloys, as well as good heat-resistance at temperatures up to 1000 °C – Al2Ti (γ=3580 kg/m3, Е=208 GPa) and Al3Ti (γ=3360 kg/m3, Е=195 GPa).
The present literature review concerns crystal lattices, structures, and homogeneity areas for intermetallic compounds of the Ti–(50–75)Al diagram, as well as thermo-physical and mechanical properties thereof.
It has been established that the metastable Al5Ti3 phase has a wide range of concentrations and is table up to a temperature of 880 °С, while the high-temperature h-Al2Ti phase is stable up to 1215 °С, and the low-temperature r-Al2Ti phase is stable at normal temperature. At temperatures above 1215 °С the h-Al2Ti phase transforms into the T
2. Kablov E.N. Innovative developments of FSUE «VIAM» SSC of RF on realization of «Strategic directions of the development of materials and technologies of their processing for the period until 2030». Aviacionnye materialy i tehnologii, 2015, no. 1 (34), pp. 3–33. DOI: 10.18577/2071-9140-2015-0-1-3-33.
3. Antipov V.V. Prospects for development of aluminium, magnesium and titanium alloys for aerospace engineering. Aviacionnye materialy i tehnologii, 2017, no. S, pp. 186–194. DOI: 10.18577/2107-9140-2017-0-S-186-194.
4. Sauthoff G. Intermetallic Phase – Materials Developments and Prospects. Zeitschrift fur Metallkunde, 1989, b. 80, h. 5, pp. 337–344.
5. Sauthoff G. Intermetallic Alloys – Overview on New Materials Developments for Structural Application in West Germany. Zeitschrift fur Metallkunde, 1990, b. 81, h. 12, pp. 855–861.
6. Carol A., Gintly A., Hugh R.G. The Application of Advanced Materials for Aircraft and Space Constractions. 24th International SAMPE Technical Conference, 1992, pp. T1029–T1093.
7. Ivanov V.I., Yasinsky K.K. Efficiency of application of heat-resistant alloys based on Ti3Al and TiAl intermetallic compounds for operation at temperatures of 600–800 °C in aerospace engineering. Tekhnologiya legkikh splavov, 1996, no. 3, pp. 7–12.
8. Aviation materials and technologies. Moscow: VIAM, 2007, is.: Combustion and fire safety of titanium alloys. 80 p.
9. Ivanov V.I., Nochovnaya N.A. Promising heat-resistant materials based on titanium aluminides. Proc. Int. scientific and technical conf. «Scientific ideas of S.T. Kishkina and modern materials science». Moscow: VIAM, 2006, pp. 98–103.
10. Kablov E.N., Nochovnaya N.A., Panin P.V., Alekseev E.B., Novak A.V. Investigation of the structure and properties of heat-resistant alloys based on titanium aluminides with microadditions of gadolinium. Materialovedeniye, 2017, no. 3, pp. 3–10.
11. Panin P.V., Nochovnaya N.A., Kablov D.E., Alekseev E.B., Shiryaev A.A., Novak A.V. A practical guide to metallography of alloys based on titanium and its intermetallic compounds: textbook. Ed. E.N. Kablov. Moscow: VIAM, 2020, 200 p.
12. Duyunova V.A., Nochovnaya N.A., Alekseev E.B., Ivanov V.I. Study of the influence of alloying and hot deformation on the properties of small-sized stampings from alloys based on the TiAl intermetallic compound. Metallurg, 2020, no. 8, pp. 83–88.
13. Bykov Yu.G., Nochovnaya N.A., Timokhin V.M., Alekseev E.B., Novak A.V., Zakharova E.S. Application of intermetallic titanium ortho-alloy in bling structure of high pressure compressor guide vanes. Elektrometallurgiya, 2019, no. 11, pp. 19–26.
14. Novak A.V., Nochovnaya N.A., Alekseev E.B. Influence of the parameters of deformation processing on the morphology of the hardening o-phase and the mechanical properties of the intermetallic titanium alloy VIT5. Deformatsiya i razrusheniye materialov, 2019, no. 6, pp. 10–16.
15. Novak A.V., Nochovnaya N.A., Alekseev E.B. Influence of rare earth elements on the structure and properties of an alloy based on orthorhombic titanium aluminide. Titan, 2019, no. 4 (66), pp. 17–23.
16. Dzunovich D.A., Alekseyev E.B., Panin P.V., Lukina E.A., Novak A.V. Structure and properties of sheet semi-finished products from various wrought intermetallic titanium alloys. Aviacionnye materialy i tehnologii, 2018, no. 2 (51), pp. 17–25. DOI: 10.18577/2071-9140-2018-0-2-17-25.
17. Alekseev Е.B., Nochovnaya N.A., Novak A.V., Panin P.V. Wrought intermetallic titanium ortho alloy doped with yttrium Part 1. Research on ingot microstructure and rheological curves plotting. Trudy VIAM, 2018, no. 6 (66), paper no. 02. Available at: http://www.viam-works.ru (accessed: December 14, 2021). DOI: 10.18577/2307-6046-2018-0-6-12-21.
18. Alexeev Е.B., Nochovnaya N.A., Novak A.V., Panin P.V. Wrought intermetallic titanium ortho alloy doped with yttrium. Part 2. Research on heat treatment effect on rolled slab microstructure and mechanical properties. Trudy VIAM, 2018, no. 12 (72), paper no. 04. Available at: http://www.viam-works.ru (accessed: December 14, 2021). DOI: 10.18577/2307-6046-2018-0-12-37-45.
19. Novak A.V., Alekseev E.B., Ivanov V.I., Dzunovich D.A. The study of the quenching parameters influence on structure and hardness of orthorhombic titanium aluminide alloy VТI-4. Trudy VIAM, 2018, no. 2, paper no. 05. Available at: http://www.viam-works.ru (accessed: December 14, 2021). DOI: 10.18577/2307-6046-2018-0-2-5-5.
20. Nochovnaya N.A., Alekseev E.B., Panin P.V., Novak A.V. Investigation of the structure and mechanical properties of the deformable intermetallic titanium alloy VIT5 doped with gadolinium. Titan, 2017, no. 2 (55), pp. 21–29.
21. Zavodov A.V., Nochovnaya N.A., Alekseev E.B., Novak A.V. Dynamics of changes in the structural-phase state during annealing of an intermetallic titanium alloy of the Ti – Al – Nb system. Titan, 2017, no. 4 (58), pp. 23–28.
22. Appel F., Oehring M. γ-Titanium Aluminide Alloys: Alloy Design and Properties. Titanium and Titanium Alloys. Fundamentals and Applications. Wiemheim: Wiley-VCH, 2003, pp. 89–152.
23. Appel F., Clemens H., Fischer F. Modeling concepts for intermetallic titanium aluminides. Journal of Progress Materials Science, 2016, vol. 81, pp. 55–124.
24. Bewlay B.P., Nag S., Suzuki A., Weimer M.J. TiAl alloys in commercial aircraft engines materials at high temperatures. Journal of Materials at High Temperatures, 2016, vol. 33, no. 5, pp. 549–559.
25. Lasalmonie A. Intermetallics: Why is its so difficult to introduce them in gas turbine engines. Journals of Intermetallics, 2006, vol. 14, pp. 1123–1129.
26. Smarsly W., Bauer H., Glitz G., Clemens H. et al. Titanium aluminides for automotive and gas turbine application. Proceeding Conference Structural Intermetallic. Warrendale: TMS, 2001, pp. 25–34.
27. Benci J.T., Ma J.C., Feist F. Evaluation of the intermetallic compound Al2Ti for elevated – temperature application. Materials Science Engineering A, 1995, vol. 192, pp. 38–44.
28. Kovneristy Y.K., Budberg P.B. Role of the Phase Diagrams for Development Titanium Alloys. Titanium`99. Science and Technology: Proceeding of the 9 th Wold Conference on Titanium. 2000, vol. 1, pp. 115–123.
29. Grystsev A., Rogl F. Reassessment of the binary aluminium–titanium phase diagram. Journals of Phase Eqiulibrium and Diffusion, 2003, vol. 24, pp. 511–527.
30. Schuster J.C., Palm M. Phase and phase relations in the partial system TiAl3–TiAl. Journals of Phase Eqiulibrium and Diffusion, 2006, vol. 27, pp. 255–277.
31. Batalu D., Cosmeleata G., Aloman A. Critical analysis of the Ti–Al phase diagrams. University Politechnica of Bucharest Scientific Bulletin, series B. 2006, vol. 68, no. 4, pp. 77–90.
32. Witusiewicz V.T., Bondar A.A., Hecht U., Rex U. et al. The Al–B–Nb–Ti system. III. Thermodynamic reevaluation of the constuent binary system Al–Ti. Journals of Alloys and Compounds, 2008, vol. 465, no. 1–2, pp. 64–77.
33. Schuster J.C., Ipser H. Phase and phase relation in the partial system TiAl3–TiAl. Zeitschrift fur Metallkunde, 1990, b. 81, h. 6, pp. 389–396.
34. Kattner U.R., Lin J.-C., Chang Y.C. Thermodynamic Assessment and Calculation of the Ti–Al system. Journal of Metallugical Transaction A, 1992, vol. 23, pp. 2081–2090.
35. Okamoto H. Al–Ti (Aluminium–Titanium). Journal of Phase Equilibrium, 1993, vol. 14, no. 1, pp. 120–123.
36. Bulanova M., Tretyachenko L., Golovkova M. Phase Equilibria in the Ti-rich corner of the Ti–Si–Al system. Zeitschrift fur Metallkunde, 1997, b. 88, h. 3, pp. 256.–265
37. Braun J., Ellner M. Phase equilibria investigations on the aluminium-rich part of the binary systens Ti–Al. Journal of Metallugical Material Transactions, 2001, vol. 32A, no. 5, pp. 1037–1047.
38. Heewing A., Palm M., Inden G. Phase equilibria in the Al–Nb–Ti system at high temperatures. Journal of Intermetallics, 1998, vol. 6, no. 2, pp. 79–94.
39. Schhmid-Fetzer R. Phase evaluations in binary Ti–Al system. NSIT Binary Evaluation Program in MSIT Workplace. Stuttgart: Materials Science International Services, 2003, pp. 39–45.
40. Nakano T., Negishi A., Hayashi K., Umakoshi Y. Ordering process of Al5Ti3, h-Al2Ti and r-Al2Ti with FCC-base long-period superstructures in rapid solidified Al-rich TiAl alloys. Journal of Acta Materialia, 1999, vol. 47, no. 4, pp. 1091–1104.
41. Nochovnaya N.A., Bazyleva O.A., Kablov D.E., Panin P.V. Intermetallic alloys based on titanium and nickel. Ed. E.N. Kablov. Moscow: VIAM, 2018. 318 p.
42. Benci J.T., Ma J.C. The mechanical behavior of and deformation mechanisms in Al2Ti. Journal of Materials Science and Engineering A, 1997, vol. 239–240, pp. 193–201.
43. Fehmi S.D., Zhang S. Super Alloys for Super Jobs. Aerospace Materials Handbook. CRC Press, 2013, pp. 1–77.
44. Milman Y.V., Miracle D.B., Chugunova S.I. et al. Mechanical behavior of Al3Ti intermetallic and L12 phase on its bases. Journal of Intermetallics, 2001, vol. 9, no. 9, pp. 839–845.
45. Hall E.L., Ritter A.M. Structure and behavior of metal/ceramic interfases in titanium alloy/SiC metal matrix composites. Journal of Materials Research, 1993, vol. 8, no. 5, pp. 1158–1168.
46. Takahashi T., Tomanaga K., Tsuchida Y. et al. Mechanical properties of L12 modifed titanium trialuminides with chromium, iron and vanadium. Journal of Materials Science and Engineering A – Structures, 2002, vol. 329–333, no. 1, pp. 474–480.
47. Kim S., Cho W., Hong C.-P. et al. Creep behavior of cast TiAl based intermetallics. Journal of Materials Science and Technology, 1995, vol. 11, no. 5, pp. 1147–1155.
48. Durlu N., Inal O.T. L12-type ternary titanium aluminides as electron concentration phases. Journal of Materials Science. 1992, vol. 27, no. 12, pp. 3225–3230.
49. Ghosh G., Van de Walle A., Asta M. First-Principles Phase Stability calculation of pseudo binary alloys of (Al, Zn)3Ti with L12, DO22 and DO33 Structures. Journal of Phase Equilibrium and Diffusion, 2007, vol. 28, no. 1, pp. 9–22.
50. Karpets M.V., Milman Y.V., Barabash O.M. et al. The influence of Zr alloying on the structure and properties of Al3Ti. Journal of Intermetallics, 2003, vol. 11, no. 3, pp. 241–249.
51. Wang S., Guo P., Yang L. et al. Microstructure and mechanical properties (Al, Cr)3Ti based alloy with different Al additions. Journal of Materials and Design, 2009, vol. 30, no. 3, pp. 704–709.
52. Mabuchi H., Morimoto H., Kakitsuji A. et al. Microstructure and mechanical properties of L12–(Al, Cr) Ti/Ti2AlN composites produced by reactive arc-melting. Journal of Scripta Materialia, 2001, vol. 44, pp. 2503–2508.
53. Tian W.H., Nemoto M. Crystallography and morphology of DO23–Al11Ti5 precipitation in Ag-modified L12–Al3Ti. Journal of Intermetallics, 2000, vol. 8, no. 8, pp. 835–843.
54. Hu H., Wu X., Wang R. et al. Structural Stability, mechanical properties and stacking fault energies of Al3Ti alloyed with Zn, Cu, Ag: Ferst-principles studied. Journal of Alloys and Compounds, 2016, vol. 666, pp. 185–196.
55. Fanag S., Solovyev I.V., Sawade H. et al. Formation of La-modified L12–Al3Ti by mechnical alloying and annealing. Journal of Materials Characterization, 2008, vol. 59, pp. 440–445.
56. Stein F., Zhang L., Sauthoff G., Palm M. TEM and DTA study on the stability of Al5Ti3 and h-Al2Ti-superstructures in aluminium-rich TiAl alloys. Journal of Acta Materialia, 2001, vol. 49, no. 15, pp. 2919–2932.
57. Zhang L., Palm M., Stein F., Sauthoff G. Formation of lamellar microstructures Al-rich TiAl alloys between 900 to 1100 °C. Journal of Intermetallics, 2001, vol. 9, pp. 229–238.
58. Palm M., Zhang L., Stein F., Sauthoff G. Phase and phase equilibria in the Al-rich part of the Al–Ti system above 900 °C. Journal of Intermetallics, 2002, vol. 10, no. 6, pp. 523–540.
59. Palm M., Engberding N., Stein F., Kelm K., Irsen S. Phase and evolution of microstructures in Ti–60 Al at. %. Journal of Acta Materialia, 2012, vol. 60, pp. 3559–3569.
60. Nakano T., Hayashi K., Umakoshi Y., Chiu Y., Veyssiere P. Effect of long-period superstructures on plastic properties in Al-rich TiAl single crystals. MRS Proceedings, 2004, vol. 842. DOI: 10.1557/PROC-842-S7.4.
61. Nakano T., Negishi A., Hayashi K., Umakoshi Y. Ordering process of Al5Ti3, h-Al2Ti and r-Al2Ti with FCC-base long-period superstructures in rapid solidified Al-rich TiAl alloys. Journal of Acta Materialia, 1999, vol. 47, no. 4. Р. 1091–1104.
62. Nakano T., Hayashi K., Nagasawa Y., Umakoshi Y. Plastic Deformation Behavior of Al5Ti3 Single-Phase Crystal. MRS Proceedings, 2002, vol. 753. DOI: 10.1557//PROC-753-BB5.8.
63. Hata S., Higuchi K., Itakura M. et al. Shot-range order in Al-rich γ-TiAl alloys studied by high-resolution transmission electron microscopy with image processing. Journal of Philosophical Magazine Letter, 2002, vol. 82, no. 7, pp. 363–372.
64. Hayashi K., Nakano T., Umakoshi Y. Metastable region of Al5Ti3 single-phase in time-temperature-transformation (TTT) diagram of Ti–62 at. % Al single crystal. Journal of Intermetallics, 2002, vol. 10, no. 8, pp. 771–781.
65. Hata S., Higuchi K., Mitate T., Kuwano N. et al. HRTEM observation of Partially Ordered Long-period Superstructures in Al-Rich TiAl alloys. MRS Proceedings, 2002, vol. 753. DOI: 10.1557/PROC-753-BB4.2.
66. Hata S., Nakano T., Higuchi K.Y., Nagasawa Y.N. et al. Semi-quantitative HRTEM for partially ordered materials: Application to Al-rich TiAl alloys. Journal of Materials Science Forum, 2003, vol. 426–432, pp. 1721–1726.
67. Hata S., Higuchi K., Mitate T., Itakura M., Tomokiyo Y. et al. HRTEM image contrast and atomistic microstructures of long-period ordered Al-rich TiAl alloys. Journal of Electronic Microscopy, 2000, vol. 53, no. 1, pp. 1–9.
68. Sturm D., Heimaier H., Saage H., Agular J. et al. Creep strength of a binary Al62Ti38 alloy. International Journal Materials Research, 2010, vol. 101, no. 5, pp. 676–679.
69. Braun J., Ellner M. Phase equilibria investigation on the aluminium-rich part of the binary system Ti–Al. Journal of Metallugical Materials Transaction A, 2001, vol. 32, no. 5, pp. 1037–1047.
70. Palm M., Engberding N., Stein F. et al. Phase and evolution of microstructures in Ti–60 at. % Al. Journal of Acta Materialia, 2012, vol. 60, pp. 3559–3569.
71. Рaninsky M., Drevermann A., Schmitz C.J. et al. Casting and properties of Al-rich Ti–Al alloys. Ti-2007: Science and Technology Proceeding International. The Japan Institute of Metals, 2007, pp. 1059–1062.
72. Кoyma T., Doi M., Naito S. Experimantal and Theoretical Investigation of the Phase Tranformation in Al-rich TiAl Intermatallic Compounds. MRS Proceedings, 2000, vol. 646. DOI: 10.1557/PROC-646-N2.2.1.
73. Nakanо T., Hata S., Hayashi K., Umakoshi Y. Some Long-period Superstructures and the Related Motion of Dislocation in Al-rich TiAl single Crystals. Supplemental Proceedings: Materials Properties, Characterization, and Modeling, 2012, vol. 2, pp. 797–804.
74. Li J., Weng G. Time-dependent creep of a dual-phase viscoplastic material with lamellar structure. International Journal of Plastisity, 1998, vol. 14, no. 8, pp. 755–770.
75. Kad B., Hazzledine P., Fraser H. Lamellar interface and their construction to plastic flow anisotropy in TiAl-base alloys. MRS Proceeding, 1992, vol. 288, pp. 495–500.
76. Marketz W., Fischer F., Clemens H. Deformation mechanisms in TiAl intermetallics experiments and modeling. International Journal of Plastisity, 2003, vol. 19, no. 3, pp. 281–321.
77. Feng Q., Whang S. Deformation of Ti–56 at. % Al single oriented for single slip by 1/2<110] ordinary dislocations. Journal of Acta Materialia, 2000, vol. 48, no. 17, pp. 4307–4321.
78. Sturm D., Heilmaier M., Saage H. et al. Creep strength of binary Al62Ti38 alloy. Journals of Physics, 2010, vol. 240. DOI: 10.1088/1742-6596/240/1/012084.
79. Inui H., Matsumoto M., Wu D., Yamagushi M. Temperature dependence of yield stress, deformation mode and deformation structure in single crystals of TiAl (Ti–56 at. % Al). Journal of Philosophical Magazine A, 1997, vol. 75, no. 2, pp. 395–423.
80. Jiao S., Bird N., Hirsh P.B., Taylor G. Yield stress anomalies in single crystals of Ti–54,3 at. % Al. II. ½[112] (111) slip. Journal of Philosophical Magazine A, 1998, vol. 78, no. 3, pp. 777–802.
81. Nakano T., Matsumoto K., Seno T., Umakoshi Y. Effect of chemical ordering on the deformation mode of Al-rich Ti-single crystals. Journal of Philosophical Magazine A, 1996, vol. 74, no. 1. P. 251–268.
82. Hayashi K., Nakano K., Umakoshi Y. Plastic deformation behavior and deformation substructure in Al-rich TiAl single crystals deformed at high temperatures. Journal of Science Technology and Advanced Materials, 2001, no. 2, pp. 433–441.
83. Kawabata T., Kanai T., Izumi O. Dislocation structures of a TiAl single crystal with the [110] orientation deformed at 1073 K. Journal of Philosophical Magazine A, 1994, vol. 70, no. 1, pp. 43–51.
84. Viguir B., Hemker K., Bonnevilli J. et al. Modeling the flow stress anomaly in γ-TiAl experimental observations of dislocation mechanisms. Journal of Philosophical Magazine A, 1995, vol. 71, no. 6, pp. 1295–1312.
85. Nakano T., Hayashi K., Ashida K., Umakoshi Y. Effect of Al2Ti Phase on plastic Behavior in Ti‒62.5 at. % Al Single Crystals. MRS Online Proceedings Library, 1998, vol. 552. Available at: www.cambridge.org (accessed: February 15, 2021). DOI: 10.1557//Proc-552-KK5.9.1.
86. Nakano T., Hayashi K., Umakoshi Y. et al. Effect of Al concentration and resulting long-period super structures on the plastic properties at room temperature of Al-rich TiAl single crystals. Journal of Philosophical Magazine A, 2005, vol. 85, no. 22, pp. 2527–2548.
87. Gregori F., Veyssiere P. Planar debris in plastically deformed Al-rich γ-TiAl. Journal of Philosophical Magazine A, 1999, vol. 79, no. 2, pp. 403–421.
88. Umakoshi Y., Nagano T., Ashida K. High-temperature deformation in Ti–62,5 at. % Al single crystals containing small Al2Ti-type precipitates. Journal of Materials Science Forum, 1999. Vol. 304–306, pp. 1467–1476.
89. Jiao S., Bird N., Hirsh P.B., Taylor G. Yield stress anomalies in single crystals of Ti–54,5 at. % Al. III. Ordinary slip. Journal of Philosophical Magazine A, 2001, vol. 81, no. 1, pp. 213–244.
90. Lei C., Xu Q., Sun Y.Q. TEM Investigation of Interfaces between Ti3Al5 and TiAl2. Journal of Phisica Status Soliditi A, 2000, vol. 179, no. 1, pp. 77–82.
91. Fabienne G., Veyssiere P. Microstructures in Al-rich γ-TiAl strained in the domain of temperature of flow stress anomalies. Bulletin of Materials Science, 1999, vol. 22. No 3, pp. 585–592.
92. Appel F., Paul J.D.H., Oehring M. Application, Component Assessment, and Outlook. Gamma Tutanium Aluminide Alloys: Science and Technology. Weinheim: Wiley-VCH Verlag, 2011. P. 729–738.
93. Gregori F., Veyssiere P. A microstructural analysis of Al-rich γ-TiAl deformed by <011] dislocations. Journal of Materials Science Engineering A, 2001, vol. 309–310, pp. 87–91.
94. Nakano T., Hayashi K., Umakoshi Y. Formation and stability of transitional long-period superstructures in Al-rich TiAl single crystals. Journal of Philosophical Magazine A, 2002, vol. 82. P. 763–777.
95. Lei C., Xu Q., Sun Y. Phase orientation relationships in the TiAl–TiAl2 region. Journal of Materials Science Engineering A, 2001, vol. 313, pp. 227–236.
96. Inui H., Chikudo K., Nomura K., Yamagushi M. Lattice defects and their influence on the deformation behaviour of single crystals of TiAl. Journal of Materials Science Engineering A, 2002, vol. 329–331, pp. 377–387.
97. Gregori F., Veyssiere P. Properties of <011] slip in Al-rich γ-TiAl. I Dissociation, locking and decomposition of <011] dislocations at room temperature. Journal of Philosophical Magazine A, 2000, vol. 80, no. 12, pp. 2913–2932.
98. Umakoshi Y., Nakano T., Ashida K. High-temperature deformation in Ti–62,5 at. % Al single crystals containing small Al2Ti-type precipitates. Journal of Materials Science Forum, 1999. Vol. 304–306, pp. 163–168.
99. Feng Q., Wang S. Cross-slip and glide behavior of ordinary dislocations in single crystal γ-Ti–56 Al. Journal of Intermetallics, 1999, vol. 7, no. 9, pp. 971–979.
The development of additive technologies (AT) and the industrial «Internet of things» is one of the key factors that will determine the transition to the concept of «Industry 4.0». In particular, the «Internet of Things» presupposes the presence of connections between various devices and the center in which these devices will be produced as needed (resource development, the impact of operational loads exceeding the design ones). To ensure such communication, the devices or parts that make up it must have built-in sensors that will monitor the parameters of the functional state and transmit the necessary information.
This approach should be based on the development of completely new «smart» materials that combine a high level of physical and mechanical properties with a set of functional characteristics that were not previously characteristic of them.
The paper provides an overview of the research results in the field of obtaining functional materials by layer-by-layer fusion of filled polymers (FDM printing). It is shown that the use of FDM printing of polymer composites with various functional fillers makes it possible to impart electro-thermal-conductive and magnetic properties to polymer materials. By varying the composition of the polymer matrix, the type of filler, the electrical conductivity of the composite can be changed from 10-2 to 1.4·105 C/cm, the thermal conductivity can be increased to 0.9 W/mK⁰, and magnetoplastics can be produced. However, to obtain a high level of functional properties, it is required to use polymer matrices with a filling degree of 5-50%.
The combination of fundamental knowledge accumulated in the study of the structure and properties of polymer matrices filled with particles and fibers of nano- and micro-size with&
2. Kablov E.N. The dominant feature of the national technology initiative. Problems of accelerating the development of additive technologies in Russia. Metally Evrazii, 2017, no. 3, pp. 2–6.
3. Kablov E.N. Innovative developments of FSUE «VIAM» SSC of RF on realization of «Strategic directions of the development of materials and technologies of their processing for the period until 2030». Aviacionnye materialy i tehnologii, 2015, no. 1 (34), pp. 3–33. DOI: 10.18577/2071-9140-2015-0-1-3-33.
4. Kablov E.N. New generation materials – the basis of innovation, technological leadership and national security of Russia. Intellekt i tekhnologii, 2016, no. 2 (14), pp. 16–21.
5. Pavlyuk B.Ph. The main directions in the field of development of polymeric functional materials. Aviacionnye materialy i tehnologii, 2017, no. S, pp. 388–392. DOI: 10.18577/2071-9140-2017-0-S-388-392.
6. Terekhov I.V., Shlenskiy V.A., Kurshev E.V., Lonskiy S.L., Dyatlov V.A. Researches of factors affecting the formation of epoxy-containing microcapsules for the self-healing compositions. Aviacionnye materialy i tehnologii, 2018, no. 3 (52), pp. 27–34. DOI: 10.18577/2071-9140-2018-0-3-27-34.
7. Perov N.S. Design of polymeric materials on the molecular principles. II. The molecu-lar mobility in the cross-linked complex systems. Aviacionnye materialy i tehnologii, 2017, no. 4 (49), pp. 30–36. DOI: 10.18577/2071-9140-2017-0-4-30-36.
8. Kondrashov S.V., Shashkeev K.A., Petrova G.N., Mekalina I.V. Constructional polymer composites with functional properties. Aviacionnye materialy i tehnologii, 2017, no. S, pp. 405–419. DOI: 10.18577/2071-9140-2017-0-S-405-419.
9. Khosravani M.R., Reinicke T. Applications of additive manufacturing in fabrication of sensors-A review. Sensors and Actuators A: Physical, 2020, vol. 305, no. 4, pp. 111916.
10. Kondrashov S.V., Pykhtin A.A., Larionov S.A., Sorokin A.E. Influence of the technological FDM-modes of the press and structure of used materials on physic-mechanical cha-racteristics of FDM-models (review). Trudy VIAM, 2019, no. 10 (82), paper no. 04. Available at: http://www.viam-works.ru (accessed: February 22, 2020). DOI: 10.18577/2307-6046-2019-0-10-34-49.
11. Popescu D., Zapciu A., Amza C. et al. FDM process parameters influence over the mechanical properties of polymer specimens: A review. Polymer Testing, 2018, vol. 69, pp. 157–166.
12. Ngo T.D., Kashani A., Imbalzano G. et al. Additive manufacturing (3D printing): A review of materials, methods, applications and challenges. Composites Part B: Engineering, 2018, vol. 143, pp. 172–196.
13. Lipatov Yu.S. Interfacial phenomena in polymers. Kiev: Naukova Dumka, 1980, 260 p.
14. Kondrashov S.V., Shashkeev K.A., Popkov O.V., Solovyanchik L.V. Prospective producing methods for functional structural materials based on CNT-filled nanocomposites (review). Trudy VIAM, 2016, no. 3 (39), paper no. 07. Available at: http://www.viam-works.ru (accessed: December 10, 2020). DOI: 10.18577/2307-6046-2016-0-3-7-7.
15. Kondrashov S.V., Shashkeev K.A., Popkov O.V., Solovyanchik L.V. Mechanical properties of CNT nanocomposites (review). Trudy VIAM, 2016, no. 5 (41), paper no. 08. Available at: http://www.viam-works.ru (accessed: December 10, 2020). DOI: 10.18577/2307-6046-2016-0-5-8-8.
16. Sezer H.K., Eren O. FDM 3D printing of MWCNT re-inforced ABS nano-composite parts with enhanced mechanical and electrical properties. Journal of Manufacturing Processes, 2019, vol. 37, pp. 339–347.
17. Alig I., Lellinger D., Skipa T. Influence of thermo-rheological history on electrical and rheological properties of polymer–carbon nanotube composites. Polymer–Carbon Nanotube Composites, Woodhead Publishing, 2011, pp. 295–328.
18. Shante V.K.S., Kirkpatrick S. An introduction to percolation theory. Advances in Physics, 1971, vol. 20, no. 85, pp. 325–357.
19. Sorokin A.E., Pykhtin A.A., Larionov S.A., Belyaev A.A., Lonsky S.L., Kondrashov S.V., Lobanov M.V. et al. Structure and properties of CNT modified filaments based on ABS plastic. Vse materialy. Entsiklopedicheskiy spravochnik, 2020, no. 4, pp. 1–16.
20. Jyoti J., Basu S., Singh B.P. et al. Superior mechanical and electrical properties of multiwall carbon nanotube reinforced acrylonitrile butadiene styrene high performance composites. Composites Part B: Engineering, 2015, vol. 83, pp. 58–65.
21. Vacha J., Borůvka M. Mechanical properties of acrylonitrile butadiene styrene thermoplastic polymer matrix with carbon nanotubes. NANOCON, 2015. Available at: http://www.nanocon.eu/files/proceedings/23/index_en.htm (accessed: november 27, 2020).
22. Villmow T., Pegel S., Pötschke P. et al. Influence of injection molding parameters on the electrical resistivity of polycarbonate filled with multi-walled carbon nanotubes. Composites Science and Technology, 2008, vol. 68, no. 3–4, pp. 777–789.
23. Tiusanen J., Vlasveld D., Vuorinen J. Review on the effects of injection moulding parameters on the electrical resistivity of carbon nanotube filled polymer parts. Composites Science and Technology, 2012, vol. 72, no. 14, pp. 1741–1752.
24. Yang L., Li S., Zhou X., Liu J. et al. Effects of carbon nanotube on the thermal, mechanical, and electrical properties of PLA/CNT printed parts in the FDM process. Synthetic Metals, 2019. Vol. 253, pp. 122–130.
25. Spinelli G., Lamberti P., Tucci V. et al. Rheological and electrical behaviour of nanocarbon/poly (lactic) acid for 3D printing applications. Composites Part B: Engineering, 2019, vol. 167, pp. 467–476.
26. Yu W.W., Zhang J., Wu J.R. et al. Incorporation of graphitic nano-filler and poly (lactic acid) in fused deposition modeling. Journal of Applied Polymer Science, 2017, vol. 134, no. 15, p. 44703.
27. Postiglione G., Natale G., Griffini G. et al. Conductive 3D microstructures by direct 3D printing of polymer/carbon nanotube nanocomposites via liquid deposition modeling. Composites Part A: Applied Science and Manufacturing, 2015, vol. 76, pp. 110–114.
28. Chizari K., Arjmand M., Liu Z. et al. Three-dimensional printing of highly conductive polymer nanocomposites for EMI shielding applications. Materials Today Communications, 2017, vol. 11, pp. 112–118.
29. Kotsilkova R., Petrova-Doycheva I., Menseidov D. et al. Exploring thermal annealing and graphene-carbon nanotube additives to enhance crystallinity, thermal, electrical and tensile properties of aged poly(lactic)acid-based filament for 3D printing. Composites Science and Technology, 2019, vol. 181, p. 107712.
30. Gnanasekaran K., Heijmans T., Van Bennekom S. et al. 3D printing of CNT-and graphene-based conductive polymer nanocomposites by fused deposition modeling. Applied Materials Today, 2017, vol. 9, pp. 21–28.
31. Ye W., Wu W., Hu X. et al. 3D printing of carbon nanotubes reinforced thermoplastic polyimide composites with controllable mechanical and electrical performance. Composites Science and Technology, 2019, vol. 182, pp. 107671.
32. Wei X., Li D., Jiang W., Gu Z. et al. 3D printable graphene composite. Scientific reports, 2015, vol. 5, pp. 11181.
33. Singh R., Sandhu G.S., Penna R. et al. Investigations for thermal and electrical conductivity of ABS-graphene blended prototypes. Materials, 2017, vol. 10, no. 8, pp. 881–890.
34. Leigh S.J., Bradley R.J., Purssell C.P. et al. A simple, low-cost conductive composite material for 3D printing of electronic sensors. PloS one, 2012, vol. 7, no. 11. DOI: 10.1371/journal.pone.0049365.
35. Kwok S.W., Goh K.H.H., Tan Z.D. et al. Electrically conductive filament for 3D-printed circuits and sensors. Applied Materials Today, 2017, vol. 9, pp. 167–175.
36. Cruz M.A., Ye S., Kim M.J. et al. Multigram synthesis of Cu–Ag Core–shell nanowires enables the production of a highly conductive polymer filament for 3D printing electronics. Particle & Particle Systems Characterization, 2018, vol. 35, no. 5, pp. 1700385.
37. Tan J.C., Low H.Y. Embedded electrical tracks in 3D printed objects by fused filament fabrication of highly conductive composites. Additive Manufacturing, 2018, vol. 23, pp. 294–302.
38. Lei Z., Chen Z., Peng H. et al. Fabrication of highly electrical conductive composite filaments for 3D-printing circuits. Journal of Materials Science, 2018, vol. 53, no. 20, pp. 14495–14505.
39. Pang H., Xu L., Yan D.X. et al. Conductive polymer composites with segregated structures. Progress in Polymer Science, 2014, vol. 39, no. 11, pp. 1908–1933.
40. Iron-filled Metal Composite PLA. Available at: https://www.proto-pasta.com/products/magnetic-iron-pla (accessed: November 27, 2020).
41. Bollig L.M., Hilpisch P.J., Mowry G.S. et al. 3D printed magnetic polymer composite transformers. Journal of Magnetism and Magnetic Materials, 2017, vol. 442, pp. 97–101.
42. Chernavsky P.A., Pankina G.V., Lunin V.V. Methodological developments for practical work on the special course «Methods of magnetometry in heterogeneous catalysis». Moscow: Moscow State University. M.V. Lomonosov, 2017, pp. 19–21.
43. Khatri B., Lappe K., Noetzel D. et al. A 3D-printable polymer-metal soft-magnetic functional composite – Development and characterization. Materials, 2018, vol. 11, no. 2, pp. 189–201.
44. Palmero E.M., Rial J., de Vicente J. et al. Development of permanent magnet MnAlC/polymer composites and flexible filament for bonding and 3D-printing technologies. Science and Techno-logy of advanced Materials, 2018, vol. 19, no. 1, pp. 465–473.
45. Huber C., Abert C., Bruckner F. et al. 3D Printing of Polymer Bonded Rare-Earth Magnets With a Variable Magnetic Compound Density for a Predefined Stray Field. Available at: https://www.nature.com/articles/s41598-017-09864-0 (accessed: November 27, 2020).
46. Jabr R.A. Application of geometric programming to transformer design. IEEE Transactions on Magnetics, 2005, vol. 41, no. 11, pp. 4261–4269.
47.Leigh S.J., Purssell C.P., Billson D.R. et al. Using a magnetite/thermoplastic composite in 3D printing of direct replacements for commercially available flow sensors. Smart materials and structures, 2014, vol. 23, no. 9, pp. 095039.
48.Gubin S.P., Koksharov Yu.A., Khomutov G.B., Yurkov G.Yu. Magnetic nanoparticles: methods of preparation, structure and properties. Uspekhi khimii, 2005, vol. 74, no. 6, pp. 539–574.
49. Arie M.A., Shooshtari A.H., Tiwari R. et al. Experimental characterization of heat transfer in an additively manufactured polymer heat exchanger. Applied Thermal Engineering, 2017, vol. 113, pp. 575–584.
50. Hymas D.M., Arie M.A., Singer F. et al. Enhanced air-side heat transfer in an additively manufactured polymer composite heat exchanger. 16th IEEE Intersociety Conference on Thermal and Thermomechanical Phenomena in Electronic Systems (ITherm). 2017, pp. 634–638.
51. Nikzad M., Masood S.H., Sbarski I. Thermo-mechanical properties of a highly filled polymeric composites for fused deposition modeling. Materials & Design, 2011, vol. 32, no. 6, pp. 3448–3456.
52. Hwang S., Reyes E.I., Moon K.S. et al. Thermo-mechanical characterization of metal/polymer composite filaments and printing parameter study for fused deposition modeling in the 3D printing process. Journal of Electronic Materials, 2015, vol. 44, no. 3, pp. 771–777.
53. Quill T.J., Smith M.K., Zhou T. et al. Thermal and mechanical properties of 3D printed boron nitride–ABS composites. Applied Composite Materials, 2018, vol. 25, no. 5, pp. 1205–1217.
54. Waheed S., Cabot J.M., Smejkal P. et al. Three-Dimensional Printing of Abrasive, Hard, and Thermally Conductive Synthetic Microdiamond–Polymer Composite Using Low-Cost Fused De- position Modeling Printer. ACS applied materials & interfaces, 2019, vol. 11, no. 4, pp. 4353–4363.
55. Jia Y., He H., Geng Y. et al. High through-plane thermal conductivity of polymer based product with vertical alignment of graphite flakes achieved via 3D printing. Composites Science and Technology, 2017, vol. 145, pp. 55–61.
Broad application in the aviation industry is found by glue of cold curing VK-9, and also film VK-36 glue and its updatings.
Working off of technological parameters of manufacturing of glues of the VK-9 brands is carried out and
R serial equipment of VIAM Federal State Unitary Enterprise. In the course of work parameters of technological process of preparation of initial components, and also technological process of combination of components when manufacturing glues varied.
On the equipment of VIAM Federal State Unitary Enterprise works on working off and choice of technological parameters of manufacturing of the glue masses intended for manufacturing of glue films of the brands VK-36, VK-36P, VK-36rt.140 and VK-36rt.170 are carried out and the technological instruction on their manufacturing is made.
Properties of glued joints of the D16AT aluminum alloy made using VK-9 glue with use of components from different suppliers, at temperatures of testing of 20, 80 and 125 °C in initial condition completely correspond to technical requirements of TU 1-595-14-842-2009. Glued joints maintain influence of modes of thermoageing at 200 °C – 500 h and 250 °C during 5 h with preservation of durability of glued joints as at temperature of 20 °C, and 200 °C and 250 °C.
Glue masses on the serial equipment of VIAM Federal State Unitary Enterprise are made and with their use experimental batches of film glues VK-36, VK-36P, VK-36rt.140 are received,
R Glue masses and film glues according to the characteristics completely correspond to TU 1-595-389-96 (VK-36 and VK-36P) and TU 1-595-14-486-2013 (VK-36RT.140 and VK-36RT.170).
The wide range glue binding which production
2. Kablov E.N. The strategic directions of development of materials and technologies of their processing for the period to 2030. Aviacionnye materialy i tehnologii, 2012, no. S, pp. 7–17.
3. Grashhenkov D.V., Chursova L.V. Strategy of development of composite and functional materials. Aviacionnye materialy i tehnologii, 2012, no. S, pp. 231–242.
4. Petrova A.P., Malysheva G.V. Adhesives, adhesive binders and adhesive prepregs. Ed. E.N. Kablov. Moscow: VIAM, 2017, 472 p.
5. Petrova A.P., Donskoy A.A., Chalykh A.E., Shcherbina A.A. Adhesive materials. Sealants: a reference book. Saint Peterburg: Professional, 2008. 589 p.
6. Sharova I. A. Domestic and foreign experience in area of cold curing epoxy adhesive development. Trudy VIAM, 2014, no. 7, paper no. 05. Available at: http://viam-works.ru (accessed: October 21, 2020). DOI: 10.18577/2307-6046-2014-0-7-5-5.
7. Sharova I.A. Epoxy cold curing adhesives for bonding and repairing aircraft parts: thesis abstract, Cand. Sc. (Tech.). Moscow: VIAM, 2015, 26 p.
8. Sharova I.A., Lukina N.F., Aleksashin V.M., Antyufeeva N.V. Influence of the composition on the kinetic and strength properties of rapidly hardening epoxy adhesive compositions. Klei. Germetiki. Tekhnologii, 2015, no. 2, pp. 1–5.
9. Petrova A.P. Foaming adhesives and their use in aircraft construction. Klei. Germetiki. Tekhnologii, 2015, no. 1, pp. 2–5.
10. Petrova A.P., Lukina N.F. Foaming adhesives. Klei. Germetiki. Tekhnologii, 2006, no. 9, pp. 2–5.
11. Lukina N.F., Petrova A.P., Muhametov R.R., Kogtjonkov A.S. New developments in the field of adhesive aviation materials. Aviacionnye materialy i tehnologii, 2017, no. S, pp. 452–459. DOI: 10.18577/2071-9140-2017-0-S-452-459.
12. Dementyeva L.A., Kutsevich K.E., Lukina N.F., Petrova A.P. Properties of epoxy structural adhesives modified with polysulfones. Klei. Germetiki. Tekhnologii, 2016, no. 11, pp. 13–18.
13. Kablov E.N., Chursova L.V., Lukina N.F., Kutsevich K.E., Rubtsova E.V., Petrova A.P. Investigation of epoxy-polysulfone polymer systems as a basis for high-strength adhesives for aviation purposes. Sealants. Technologies. 2017, no. 3, pp. 7–12.
14. Petrova A.P., Dementyeva L.A., Lukina N.F., Anikhovskaya L.I. Film construction adhesives. Klei. Germetiki. Tekhnologii, 2014, no. 10, pp. 7–12.
15. Lukina N.F., Dementeva L.A., Petrova A.P., Anihovskaya L.I. Gluing materials in the design of blades of helicopters. Trudy VIAM, 2016, no. 7, paper no. 07. Available at: http://www.viam-works.ru (accessed: November 6, 2021). DOI: 10.18577/2307-6046-2016-0-7-7-7.
16. Lukina N.F., Dementeva L.A., Petrova A.P., Serezhenkov A.A. Constructional and heat-resistant glues. Aviacionnye materialy i tehnologii, 2012, no. S, pp. 328–335.
17. Lukina N.F., Dementyeva L.A., Petrova A.P., Tyumeneva T.Yu. Properties of adhesives and adhesives for aircraft products. Klei. Germetiki. Tekhnologii, 2009, no. 1, pp. 14–24.
18. Petrova A.P., Lukina N.F., Dementyeva L.A., Tyumeneva T.Yu., Avdonina I.A., Zhadova N.S. Adhesives for aviation technology. Rossiyskiy khimicheskiy zhurnal, 2010, vol. LIV, no.1, pp. 46–52.
19. Rubtsova E.V., Sharova I.A., Petrova A.P. High-strength film adhesive VK-36T based on epoxy-polysulfone system. Novosti materialovedeniya. Nauka i tekhnika, 2016, no. 6, paper no. 08. URL: http://materialsnews.ru (accessed: October 13, 2020)
20. Kutsevich K.E., Dementyeva L.A., Lukina N.F., Chursova L.V. Properties and purposes of VK-36RM glue for aviation technology. Klei. Germetiki. Tekhnologii, 2013, no. 8, pp. 5–6.
21. Kutsevich K.E. Adhesive prepregs and carbon composites based on them: thesis, Cand. Sc. (Tech.). Moscow: VIAM, 2014, 102 p.
22. Lukina N.F., Dementeva L.A., Kutsevich K.E. Adhesive prepregs based on tissue Porsher – perspective materials for parts and units out of polymeric composite materials. Trudy VIAM, 2014, no. 6, paper no. 10. Available at: http://www.viam-works.ru (accessed: October 13, 2020). DOI: 10.18577/2307-6046-2014-0-6-10-10.
23. Petrovа A.P., Dementyevа L.A., Lukina N.F., Chursova L.V. Adhesive binders for polymer composite materials based on carbon- and glass fillers. Trudy VIAM, 2015, no. 9, paper no. 11. Available at: http://www.viam-works.ru (accessed: October 19, 2020). DOI: 10.18577/2307-6046-2015-0-9-11-11.
The article provides an overview of foreign scientific and technical literature in the field of hybrid metal matrix composites (MCM) based on aluminum alloys. The paper presents hybrid MМСs based on aluminum alloys with reinforcing components. The main methods for the manufacture of hybrid MMCs based on an aluminum alloy are liquid-phase: impregnation under pressure, casting with stirring, solid-phase: methods of powder metallurgy. Also methods of additive technology are described in the literature.
The most common aluminum alloys used for the manufacture of hybrid MMCs are alloys of grades 359, 1060, 2024, 2124, 6061, 6351, 7075. The following components and their mixtures are used for their reinforcement: silicon carbide with powders: titanium dioxide, boron carbide, nitride silicon, aluminum oxide; with metal particles: titanium, chromium. The use of silicon carbide whiskers, short fibers of aluminum oxide, nitilone fibers, and graphite particles is also noted.
The following systems of hybrid MMCs are considered: Al/TiO2–SiC, Al/SiC–B4C, Al/NiTif–SiCp, Al/SiCp–Crp, Al/SiС–Ti, Al/SiC–Si3N4, Al/SiCw–SiCp, Al/SiCw–SiCp, Al/SiCp–Gr, Al/Al2O3–C.
Data are presented on the effect of the volume or mass percentage of reinforcing components in hybrid MMCs on mechanical, thermophysical, tribological properties: tensile strength, bending, elongation, hardness, thermal conductivity, wear and coefficient of friction. Also provides information on the study of damping ability.
It is shown, that the combination of various types of reinforcing components makes it possible to obtain h
2. Kablov E.N. What to make the future of? New generation materials, technologies for their creation and processing – the basis of innovations. Krylya Rodiny, 2016, no. 5, pp. 8–18.
3. Kablov E.N., Valueva M.I., I.V. Zelenina, Khmelnitskiy V.V., Aleksashin V.M. Carbon plastics based on benzoxazine oligomers – perspective materials. Trudy VIAM, 2020, no. 1, paper no. 07. Available at: http://www.viam-works.ru (accessed: June 2, 2020). DOI: 10.18577/2307-6046-2020-0-1-68-77.
4. Imametdinov E.S., Valueva M.I. Сomposites for piston engines (rеview). Aviacionnye materialy i tehnologii, 2020, no. 3 (60), pp. 19–28. DOI: 10.18577/2071-9140-2020-0-3-19-28.
5. Karashaev M.M., Bazyleva O.A., Shesta- kov A.V., Ovsepyan S.V. Technological princi-ples for the development of metal composite materials reinforced with oxide and intermetallic particles. Aviacionnye materialy i tehnologii, 2020, no. 3 (60), pp. 29–36. DOI:10.18577/2071-9140-2020-0-3-29-36.
6. Antipov V.V. Prospects for development of aluminium, magnesium and titanium alloys for aerospace engineering. Aviacionnye materialy i tehnologii, 2017, no. S, pp. 186–194. DOI: 10.18577/2107-9140-2017-0-S-186-194.
7. Chawla N., Chawla K.K. Metal Matrix Composites. New York: Springer Sience+Business Media, Inc., 2006, pp. 351–379.
8. Almangour B. Additive Manufacturing of Emerging Materials. Springer, 2019, 355 p.
9. Debroy H.L., Wei J.S., Zuback T. et al. Additive manufacturing of metallic components – Process, structure and properties. Progress in Materials Science, 2018, vol. 92, pp. 112–224.
10. Venugopal S., Karikalan L. Microstructure and physical properties of hybrid metal matrix composites AA6061–TiO2–SiC via stir casting techniques. Materials Today: Proceedings, 2020, pp. 2–6. DOI:10.1016/j.matpr.2020.06.462.
11. Gowrishankar M.C., Hiremath P., Shettar M. et al. Experimental validity on the casting characteristics of stir cast aluminium composites. Journal of Materials Research and Technology, 2020, vol. 9, is. 3, pp. 3340–3347. DOI: 10.1016/j.jmrt.2020.01.028.
12. Oh K.H., Han K.S. Short-fiber/particle hybrid reinforcement: effects on fracture toughness and fatigue crack growth of metal matrix composites. Composites Science and Technology, 2007, vol. 67, is. 7–8, pp. 1719–1726. DOI: 10.1016/j.compscitech.2006.06.020.
13. Hu J., Wu G., Zhang Q., Gou H. Mechanical properties and damping capacity of SiCp/TiNif/Al composite with different volume fraction of SiC particle. Composites. Part B: Engineering, 2014, vol. 66, pp. 400–406. DOI: 10.1016/j.compositesb.2014.06.013.
14. Lu T.W., Chen W.P., Wang P. et al. Enhanced mechanical properties and thermo-physical properties of 7075Al hybrid composites reinforced by the mixture of Cr particles and SiCp. Journal of Alloys and Compounds, 2018, vol. 735, pp. 1137–1144. DOI: 10.1016/j.jallcom.2017.11.227.
15. Liu Y.X., Yang C., Chen W.P. et al. Effects of particle size and properties on the microstructures, mechanical properties, and fracture mechanisms of 7075Al hybrid composites prepared by squeeze casting. Journal of Materials Science, 2014, vol. 49, pp. 7855–7863. DOI: 10.1007/s10853-014-8496-5.
16. Chen W., Liu Y., Yang C. et al. (SiCp+Ti)/7075Al hybrid composites with high strength and large plasticity fabricated by squeeze casting. Materials Science and Engineering: A, 2014, vol. 609, pp. 250–254. DOI: 10.1016/j.msea.2014.05.008.
17. Shalaby E.A.M., Churyumov A.Y., Solonin A.N., Lotfy A. Preparation and characterization of hybrid A359/(SiC+Si3N4) composites synthesized by stir/squeeze casting techniques. Materials Science and Engineering: A, 2016, vol. 674, pp. 18–24. DOI: 10.1016/j.msea.2016.07.058.
18. Ko B.C., Yoo Y.C. The effect of aging treatment on the microstructure and mechanical properties of AA2124 hybrid composites reinforced with both SiC whiskers and SiC particles. Composites Science and Technology, 1999, vol. 59. is. 5. pp. 775–779. DOI: 10.1016/S0266-3538(98)00118-3.
19. Pandian V., Kannan S. Processing and preparation of aerospace-grade aluminium hybrid metal matrix composite in a modified stir casting furnace integrated with mechanical supersonic vibration squeeze infiltration method. Materials Today Communications, 2020, vol. 24. DOI: 10.1016/j.mtcomm.2020.101732.
20. Ahamad N., Mohammada A., Guptab P. Wear characteristics of Al matrix reinforced with Al2O3-carbon hybrid metal matrix composites. Materials Today: Proceedings, 2020, vol. 33, no. 1, p. 2–6. DOI: 10.1016/j.matpr.2020.05.739.
21. Sharma S.S., Jagannath K., Prabhu P.R. et al. Metallography & Bulk Hardness of Artificially Aged Al6061–B4C–SiC Stir Cast Hybrid Composites. Materials Science Forum Submitted, 2016, vol. 880, pp. 140–143. DOI: 10.4028/www.scientific.net/MSF.880.140.
22. Kumar J., Singh D., Kalsi N.S. et al. Comparative study on the mechanical, tribological, morphological and structural properties of vortex casting processed, Al–SiC–Cr hybrid metal matrix composites for high strength wear-resistant applications: Fabrication and characterizations. Journal of Materials Research and Technology, 2020, vol. 9, is. 6, pp. 13607–13615. DOI: 10.1016/j.jmrt.2020.10.001.
23. Shabani M., Mazahery A. Prediction of wear properties in A356 matrix composite reinforced with B4C particulates. Synthetic Metals, 2011, vol. 161, pp. 1226–1231. DOI: 10.1016/j.synthmet.2011.04.009.
24. Bayhan M., Önel K. Optimization of reinforcement content and sliding distance for AlSi7Mg/SiCp composites using response surface methodology. Materials & Design, 2010, vol. 31, is. 6, pp. 3015–3022. DOI: 10.1016/j.matdes.2009.12.049.
25. Liu Y.B., Lim S.C., Ray S., Rohatgic P.K. Friction and wear of aluminium-graphite composites: the smearing process of graphite during sliding. Wear, 1992, vol. 159, is. 2, pp. 201–205. DOI: 10.1016/0043-1648(92)90303-P.
26. Suresha S., Sridhara B.K. Wear characteristics of hybrid aluminium matrix composites reinforced with graphite and silicon carbide particulates. Composites Science and Technology, 2010, vol. 70, is. 11, pp. 1652–1659. DOI: 10.1016/j.compscitech.2010.06.013.
27. Mahdavi S., Akhlaghi F. Effect of SiC content on the processing, compaction behavior, and properties of Al6061/SiC/Gr hybrid composites. Journal of Materials Science, 2011, vol. 46, pp. 1502–1511. DOI: 10.1007/s10853-010-4954-x.
In comparison with thermosetting materials, the use of thermoplastic binders can increase the resistance to shock loads, dust and rain erosion, and reduce the risk of corrosion. toxicity and fire hazard, solve the issues of repair of defects made during the manufacture of the product, disposal of decommissioned products, etc.
However, the processing of thermoplastics requires the development of different technologies, which is associated with higher viscosity of melts and solutions, high processing temperatures, low adhesive ability and poor solubility. Of the existing methods for obtaining KTM, the most high-quality impregnation of the filler with a binder and the highest level of mechanical properties of the material provide mortar and fiber technology. It is also advisable to process composite from semi-finished products, since this technology eliminates the need to have chemical sites for the preparation of binders, impregnation of the filler and pressing of sheets to obtain the material required for this production thickness.
The most promising and less energy-intensive technologies for producing prepregs are considered to be electron-ion and molten (coating). Thus, the use of film technology for producing prepregs based on fiberglass T15(p)-76 and polysulfone PSF-150 allows produce fiberglass with a higher strength characteristics.
It is worth noting that when selecting a method of processing a KTM you need to consider design features of the product, the particular properties and technological capabilities processing the selected polymer, the conditions of operation and requirements, as well as economic factors.
2. Petrova G.N., Bader E.Ya. Structural materials based on reinforced thermoplastics. Rossiyskiy khimicheskiy zhurnal, 2010, vol. 54, no. 1, pp. 30–40.
3. Petrova G.N., Bader E.Ya. Injection molded thermoplastic materials for aerospace purposes. Rossiyskiy khimicheskiy zhurnal, 2010, vol. 54, no. 1, pp. 41–45.
4. Mukhametov R.R., Petrova A.P. Thermosetting binders for polymer composites (review). Aviacionnye materialy i tehnologii, 2019, no. 3 (56), pp. 48–58. DOI: 10.18577/2071-9140-2019-0-3-48-58.
5. Sorokin A.E., Bejder E.Ya., Izotova T.F., Nikolaev E.V., Shvedkova A.K. Investigation of carbon fiber reinforced plastic on polyphenylenesulfide resin after accelerated and natural climatic test. Aviacionnye materialy i tehnologii, 2016, no. 3 (42), pp. 66–72. DOI: 10.18577/2071-9140-2016-0-3-66-72.
6. Bondaletova L.I., Bondaletov V.G. Polymer composite materials: textbook. Tomsk: Publishing house of Tomsk Polytechnic University, 2013, 118 p.
7. Johnson R.O., Teutsch E.O. Thermoplastic aromatic polymer composites. Polymer composites, 1983, vol. 4, no. 3, pp. 162–166.
8. Johnston N.J., Clair T.L.St., Baucom R.M., Towell T.W. Polyimide Matrix Composites: Polyimidesulfone/LARC-TPI (1: 1) Blend. Tomorrow's Materials, 1989, vol. 34, pp. 976–987.
9. Kotomin S.V., Barankova T.I., Plotnikova E.L., Filippova T.N. Obtaining and properties of microplastics with polysulfone and montmorilonite. Vse materialy. Entsiklopedicheskiy spravochnik, 2016, no. 2, pp. 2–9.
10. Kotomin S.V., Ivanova R.S., Konkin A.A., Molchanov B.I. Kinetics of carbon fiber impregnation with thermoplastic melts. Khimicheskiye volokna, 1981, no. 6, pp. 29–31.
11. Kotomin S.V., Avdeev N.N. Wetting of chemical fibers with thermoplastic melts. Kolloidnyy zhurnal, 1999, vol. 61, no. 3, pp. 336–343.
12. Barantseva T.E., Gorbatkina Yu.A., Kravchenko T.P., Kerber M.L. Adhesive strength during the interaction of polyamides with aramid fibers. Khimicheskiye volokna, 1997, no. 5, pp. 51–55.
13. Bolotina L.M., Gorbatkina Yu.A., Ivanova-Mumzhieva V.G., Korneeva N.V. Influence of the molecular weight of polysulfones on their adhesion to fibers. Vysokomolekulyarnye soyedinenia, series B, 2002, vol. 44, no. 8, pp. 433–444.
14. Korneeva N.V., Gorbatkina Yu.A., Ivanova-Mumzhieva V.G. et al. Adhesion of thermoplastic matrices with different molecular weights to fibers. Mekhanika kompozitnykh materialov, 2002, vol. 38, no. 4, pp. 433–444.
15. Kablov E.N. Innovative developments of FSUE «VIAM» SSC of RF on realization of «Strategic directions of the development of materials and technologies of their processing for the period until 2030». Aviacionnye materialy i tehnologii, 2015, no. 1 (34), pp. 3–33. DOI: 10.18577/2071-9140-2015-0-1-3-33.
16. Kablov E.N. Aviation and Space Materials Science. Vse materialy. Entsiklopedicheskiy spravochnik, 2008, no. 3, pp. 2–14.
17. Kablov E.N. Chemistry in Aviation Materials Science. Rossiyskiy khimicheskiy zhurnal, 2010, vol. 54, no. 1, pp. 3–4.
18. Kablov E.N., Semenova L.V., Petrova G.N., Larionov S.A., Perfilova D.N. Polymer composite materials on a thermoplastic matrix. Izvestiya vysshikh uchebnykh zavedeniy, ser.: Chemistry and Chemical Technology, 2016, vol. 59, no. 10, pp. 61–71.
19. Petrova G.N., Beider E.Ya., Izotova T.F., Malyshenok S.V. Composite thermoplastic materials – methods of production and processing. Vse materialy. Entsiklopedicheskiy spravochnik, 2013, no. 10, pp. 10–17.
20. Tkachuk A.I., Grebeneva T.A., Chursova L.V., Panina N.N. Thermoplastic binders. The present and the future. Trudy VIAM, 2013, no. 11, paper no. 07. Available at: http://www.viam-works.ru (accessed: January 14, 2021).
21. Agafonova A.S., Kondrashov S.V. Features of a technology to manufacture monolithic glass-fiber plastics intended for radio engineering. Aviacionnye materialy i tehnologii, 2014, no. 1, pp. 30–33. DOI: 10.18577 / 2071-9140-2014-0-1-30-33.
22. Beider E.Ya., Petrova G.N., Izotova T.F. An influence of coupling agent on properties of thermoplastic glass reinforced plastics. Trudy VIAM, 2014, no. 9, paper no. 07. Available at: http://viam-works.ru (accessed: January 14, 2021). DOI: 10.18577/2307-6046-2014-0-9-7-7.
23. Beider E.Ya., Petrova G.N., Dykun M.I. Dressing of carbon fibers – fillers of thermoplastic carbon reinforced plastics. Trudy VIAM, 2014, no. 10, paper no. 03. Available at: http://www.viam-works.ru (accessed: January 14, 2021). DOI: 10.18577/2307-6046-2014-0-10-3-3.
24. Zaborskaya L.V., Yurkevich O.R., Dovgyalo V.A., Pisanova E.V. Investigation of the regularities of combining dispersed polysulfone with reinforcing fibers in the preparation of composite materials. Mekhanika kompozitnykh materialov, 1991, no. 3, pp. 403–407.
25. Ustinov V.A., Bader E.Ya. The use of composite materials with a thermoplastic matrix. Konstruktsii iz kompozitsionnykh materialov, 1991, no. 1, pp. 21–28.
26. Petrova G.N., Perfilova D.N., Gryaznov V.I., Bejder E.Ya. Thermoflexible elastomer for replacement of rubbers. Aviacionnye materialy i tehnologii, 2012, no. S, pp. 302–308.
27. Petrova G.N., Rumyantseva T.V., Perfilova D.N., Bader E.Ya., Gryaznov V.I. Thermoplastic elastomers – a new class of polymer materials. Aviacionnye materialy i tehnologii, 2010, no. 4, pp. 20–25.
28. Kryzhanovsky V.K., Burlov V.V., Panimatchenko A.D., Kryzhanovskaya Yu.V. Technical properties of polymeric materials: allowance. Saint Petersburg: Professiya, 2007, 240 p.
29. Thermoplastic compositions: pat. US 3785916; filed 11.12.70; publ. 15.01.74.
30. Treatment of carbon fiber: pat. US 4269876; filed 10.04.77; publ. 26.05.81.
31. Zaixia F., Zhangyu, Yanmo Ch., Hairu L. Tensile Properties of Glass Fiber Knitted Fabric Reinforced Polypropylene Composite Made from GF/PP Commingled Yarn Affected by Prestretching. Journal of reinforced plastics and composites, 2006, vol. 25. P. 553–560.
32. Shalin R.E., Zinoviev S.N., Pomerantseva K.P. and other Heat-resistant carbon-fiber reinforced plastic KMU-8. Aviatsionnaya promyshlennost, 1987, no. 5, pp. 10–19.
33. Nelyub V.A. Technologies for preparing prepregs. Vse materialy, 2013, no. 3, pp. 12–17.
34. Narkevich A.L., Stavrov V.P. Optimization of the modes of obtaining profiles from reinforced thermoplastics. Materialy. Tekhnologii. Instrumenty, 2003, vol. 8, no. 4, pp. 75–79.
35. Yakovlev Yu.Yu., Khasyanov R.Sh., Galiguzov A.A. et al. Peculiarities of melt flow characteristics of PERT-polyethylene filled with basalt and glass fibers. Plastichnyye massy, 2018, no. 9-10, pp. 49–51.
36. Gaitukieva Z.Kh., Akhriev A.S., Kunizhev B.I., Tkhakakhov R.B. Dielectric constant and density of polymer composites based on synthetic isoprene rubber and polyethylene containing soot and aluminum nanoparticles. Plasticheskiye massy, 2018, no. 9-10, pp. 47–49.
37. Zimin D.E. Reinforced with basalt fibers polymer composite material with increased heat and chemical resistance: thesis abstract, Cand. Sc. (Tech.). Biysk: IPKhTSO RAN, 2009, 24 p.
38. Eurasian chemical market. New polymers: polyphenylene sulfide. International business journal, 2008, vol. 39, no. 3, pp. 14–21.
39. Borodulin A.S., Kalinnikova A.N., Music S.S., Tereshkov A.G. Polyetherimides for the creation of heat-resistant polymer composite materials with high physical and mechanical properties. Vestnik Belgorodskogo gosudarstvennogo tekhnologicheskogo universiteta im. V.G. Shukhova, 2019, no. 11, pp. 94–100.
40. Ryabev A.N., Donetskiy K.I., Shaposhnikova V.V. et al. Homo- and copolyarylene ether ketones with side hydroxyl groups. Vysokomolekulyarnye soyedineniya, series B, 2009, vol. 51, no. 2, pp. 315–321.
41. Fedulov B.N., Safronov A.A., Kantor M.M., Lomov S.V. Modeling of curing of thermoplastic composites and estimation of residual stresses. Kompozity i nanostruktury, 2017, vol. 9, no. 2 (34), pp. 102–122.
With the growing use of composite materials, the automated production of parts using prepreg is of increasing interest for the creation of high-performance manufacturing. There are two main types of automation for prepreg stacking: automated strip stacking and strand stacking. However, both of these technologies are not always cost-effective for all types of parts, and manual labor is usually used to make complex parts with small production volumes. An alternative to these two dominant automation solutions is automated stacking using manipulators that grip the prepreg, transfer it to the tooling and remove the backing paper. This overview presents four different solutions for the automated placement of prepreg layers on flat surfaces that can be formed in the subsequent forming process, thus reducing system complexity. The solutions are designed for parts that today require manual layering of prepreg slabs due to technical constraints or cost considerations. These solutions have to cope with the problems caused by material properties such as the low stiffness and tackiness of the prepreg, and be able to handle a wide variety of different layer shapes. All four solutions are for prepreg which is on a rigid paper backing. The review aims to analyze and compare four solutions. It has been shown that the most versatile solution is a two-handed robot equipped with simple end grippers (manipulators). The two-handed solution allows control of prepreg gripping and placement movements that allow peel movements, which is an advantage when gripping material adhering to the manipulator's gripping surface.
2. Kablov E.N. Formation of domestic space materials science. Vestnik RFFI, 2017, no. 3, pp. 97-105.
3. Kablov E.N. VIAM: new generation materials for PD-14. Krylya Rodiny, 2019, no. 7-8, pp. 54–58.
4. Kablov E.N. Innovative developments of FSUE «VIAM» SSC of RF on realization of «Strategic directions of the development of materials and technologies of their processing for the period until 2030». Aviacionnye materialy i tehnologii, 2015, no. 1 (34), pp. 3–33. DOI: 10.18577/2071-9140-2015-0-1-3-33.
5. Doneckij K.I., Karavaev R.Yu., Raskutin A.E., Panina N.N. Properties of carbon fiber and fiberglass on the basis of braiding preforms. Aviacionnye materialy i tehnologii, 2016, no. 4 (45), pp. 54–59. DOI: 10.18577/2071-9140-2016-0-4-54-59.
6. Belinis P.G., Donetskiy K.I., Lukyanenko Yu.V., Rogozhnikov V.N., Mayer Yu., Bystrikova D.V. Volume reinforcing solid-woven preforms for manufacturing of polymer composite materials (review). Aviacionnye materialy i tehnologii, 2019, no. 4 (57), pp. 18–26. DOI: 10.18577/2071-9140-2019-0-4-18-26.
7. Gusev Yu.A., Borshhev A.V., Khrulkov A.V. Features of prepregs intended for automated laying by ATL and AFP technologies. Trudy VIAM, 2015, no. 3, paper no. 06. Available at: http://www.viam-works.ru (accessed: November 20, 2020). DOI: 10.18577/2307-6046-2015-0-3-6-6.
8. Timoshkov P.N. Equipment and materials for the technology of automated calculations prepregs. Aviacionnye materialy i tehnologii, 2016, no. 2, pp. 35–39. DOI: 10.18577/2071-9140-2016-0-2-35-39.
9. Paton R. Forming technology for thermoset composites. Composites forming technologies. Ed. A.C. Long. Cambridge: Woodhead Publishing, 2007. 328 p.
10. Lukaszewicz D.H.-J.A., Ward C., Potter K.D. The engineering aspects of automated prepreg layup: history, present and future. Composites Part B: Engineering, 2012, vol. 43 (3), pp. 997–1009.
11. Björnsson A., Jonsson M., Eklund D., Lindbäck J.E., Björkman M. Getting to grips with automated prepreg handling. Production Engineering, 2017, vol. 11 (3), pp. 1–9.
12. Mcllhagger A., Archer E., Mcllhagger R. Manufacturing processes for composite materials and components for aerospace applications. Polymer composites in the aerospace industry / ed. E.P. Irving, C. Soutis. Cambridge: Elsevier Science, 2014, 688 p.
13. Sloan J. ATL and AFP: signs of evolution in machine process control. The International Journal of High Performance Computing Applications, 2008, vol. 16 (5), pp. 1–47.
14. Newell G., Khodabandehloo K. Modelling flexible sheets for automatic handling and lay-up of composite components. The Proceedings of the Institution of Mechanical Engineers: Part B, 1995, vol. 209 (6), pp. 423–432.
15. Buckingham R.O., Newell G.C. Automating the manufacture of composite broadgoods. Composites. Part A: Applied Science and Manufacturing, 1996, vol. 27 (3), pp. 191–200.
16. Szcesny M., Heieck F., Middendorf P., Mezzacasa R., Irastorza X., Sehrschön H., Schneiderbauer M. The advanced ply placement process – an innovative direct 3D placement technology for plies and tapes. Advanced Manufacturing: Polymer & Composites Science, 2017, vol. 3, pp. 2–9.
17. Composites World: Automating the CH-53K’s composite flexbeams. Available at: https://www.compositesworld.com/articles/automating-the-ch-53ks-composite-flexbeams (accessed: November 5, 2020).
18. Curran J.P., Wright E.J., Armstrong P.J. An intelligent vacuum gripper for robotic handling. Advances in manufacturing technology II. Springer, 1987, pp. 205–209.
19. Campbell F.C. Manufacturing processes for advanced composites. Oxford: Elsevier Advanced Technology, 2004, 532 p.
20. Strong A.B. Fundamentals of composites manufacturing: materials, methods and applications. 2nd ed. Dearborn: Society of Manufacturing Engineers, 2008, 640 p.
21. Newell G.C., Buckingham R.O., Khodabandehloo K. The automated manufacture of prepreg broadgoods components – a review of literature. Composites. Part A: Applied Science and Manufacturing, 1996, vol. 27 (3), pp. 211–217.
22. Potter K. But how can we make something useful out of black string? The development of carbon fibre composites manufacturing (1965–2015). The structural integrity of carbon fiber composites: 50 years of progress and achievement of the science, development, and applications. Springer, 2017, 969 p.
23. Björnsson A., Lindbäck J.E., Johansen K. Automated removal of prepreg backing paper-a sticky problem. SAE 2013 AeroTech congress and exhibition, 2013, p. 1–9.
24. Björnsson A., Lindbäck J.E., Eklund D., Jonsson M. Low-cost automation for prepreg handling-two cases from the aerospace industry. SAE International Journal of Materials and Manufacturing. 2016, vol. 9, is. 1, pp. 68–74.
25. Björnsson A., Jonsson M., Lindbäck J.E., Akermo M., Johansen K. Robot-forming of prepreg stacks – development of equipment and methods. ECCM 2016 – Proceeding of the 17th European Conference on Composite Materials, European Conference on Composite Materials, 2016 pp. 78–85.
Currently, the use of electrochromic devices that change their optical characteristics in the composition of glazing is of great interest in various fields of industry: construction, auto and aircraft construction. The main purpose of electrochromic glazing of aircraft and cars is to increase the comfort of passengers by reducing the intensity of the passage of sunlight. The use of electrochromic glass in the structures of office and residential buildings allows you to reduce energy costs for air conditioning in summer and heating in winter.
From the point of view of energy efficiency of such devices, research aimed at developing methods for applying electrochromic materials and improving their characteristics is promising.
The paper presents a review of the literature on materials of nanostructured inorganic electrochromic coatings and methods for their preparation. The properties of metal oxides that are currently used in electrochromic devices are described. Thin coatings of NiO have a strong electrochromic effect, but they exhibit low reliability during long cycling. TiO2-based coatings
show good cycling during staining and return to their original state, but have a low color change rate and low efficiency compared to other metal oxides. WO3 coatings have the shortest staining time with varying voltage and the highest staining efficiency, long-lasting color memory effect, good contrast and cyclic stability, so they are the most promising material for use in electrochromic applications. devices. It is also shown that the creation of a nanostructured surface makes it possible to use the specific surface as efficiently as possible, as well as to increase the response rate of electrochromic devices.
2. Schwartz M. Encydopedia of smart materials. New York: John Wiley and Sons Inc., 2002, 1193 c.
3. Kablov E.N. New generation materials – the basis of innovation, technological leadership and national security of Russia. Intellekt i tekhnologii, 2016, no. 2 (14), pp. 16–21.
4. Kablov E.N. What to make the future of? New generation materials, technologies for their creation and processing – the basis of innovations. Krylya Rodiny, 2016, no. 5, pp. 8–18.
5. Kablov E.N., Semenova L.V., Bogatov V.A., Mekalina I.V. and other New electrically heated and bird-resistant polymer glazing of aircraft. Plasticheskiye massy, 2017, no. 5-6, pp. 48–52.
6. Kondrashov S.V., Shashkeev K.A., Petrova G.N., Mekalina I.V. Constructional polymer composites with functional properties. Aviacionnye materialy i tehnologii, 2017, no. S, pp. 405–419. DOI: 10.18577/2071-9140-2017-0-S-405-419.
7. Kobasnyan S.S., Anisimov I.A. Intelligent system for regulating the level of light transmission of car glasses. Zhurnal mekhaniki XXI veka, 2012, no. 11, pp. 298–299.
8. Kotok V., Kovalenko V., Solovov V., Yurlova O. The determination of electrolyte stability and conditions for electrochromic WO3 films deposition. Technology audit and production reserves, 2017, vol. 3, no. 3 (35), pp. 17–22.
9. Kotok V., Kovalenko V. The electrochemical cathodic template synthesis of nickel hydroxide thin films for electrochromic devices: role of temperature. Eastern-European Journal of Enterprise Technologies, 2017, no. 2 (11), pp. 28–34.
10. Somani P.R., Radhakrishnan S. Electrochromic materials and devices: present and future. Materials chemistry and physics, 2003, vol. 77, no. 1, pp. 117–133.
11. Mortimer R. J. Electrochromic materials. Chemical Society Reviews, 1997, vol. 26, no. 3, pp. 147-156.
12. Kablov E.N. Innovative developments of FSUE «VIAM» SSC of RF on realization of «Strategic directions of the development of materials and technologies of their processing for the period until 2030». Aviacionnye materialy i tehnologii, 2015, no. 1 (34), pp. 3–33. DOI: 10.18577/2071-9140-2015-0-1-3-33.
13. Exarkhos G.J., Zhou X.-D. Discovery-based. Design of Transparent Conducting Oxide Films. Thin Solid Films, 2007, vol. 7025, pp. 515–521.
14. Song X., Dong G., Xiao Y. et al. Properties of NiOx and its influence upon all-thin-film ITO/NiOx/ LiTaO3/WO3/ITO electrochromic devices prepared by magnetron sputtering. Vacuum, 2015, vol. 111, pp. 48–54.
15. Mortimer R. J. Electrochromic materials. Annual Review of Materials Research, 2011, vol. 41, pp. 241–268.
16. Prokopovich P.V., Kirillova E.S. Prospects for the use of a cellulose matrix as a solid polymer electrolyte for photo- and electrochromic devices. Trudy Kolskogo nauchnogo tsentra RAN, 2018, vol. 9, no. 2-2, pp. 1–6.
17. Bogatov V.A., Krynin A.G., Popkov O.V., Khokhlov Yu.A. Influence of biaxial strain on the properties of the transparent conductive coating deposited on PET film by reactive magnetron sputtering. Trudy VIAM, 2016, no. 1 (37), paper no. 6. Available at: http://www.viam-works.ru (accessed: December 17, 2020). DOI: 10.18577/2307-6046-2016-0-1-42-49.
18. Gorjanca T.C., Leonga D., Py C., Rotha D. Room temperature deposition of ITO using r.f. magnetron sputtering. Thin Solid Films, 2002, vol. 413, pp. 181–185.
19. Bogatov V.A., Krynin A.G., Shchur P.A. Influence of the leakage value in the vacuum chamber on the parameters of reactive magnetron discharge and properties of titanium oxide coatings. Aviacionnye materialy i tehnologii, 2019, no. 1 (54), pp. 17–22. DOI: 10.18577/2071-9140-2019-0-1-17-22.
20. Kuzmichev A.I. Magnetron sputtering systems. Introduction to physics and technology of magnetron sputtering. Kiev: Avers, 2008, 244 p.
21. Elinson V.M., Shchur P.A., Lyamin A.N. Nanostructuring of the Polyethyleneterephthalate Surface Using Ion-Plasma Technology with the Help of Fluorine-Containing Gas Mixtures. High Temperature Material Processes: An International Quarterly of High-Technology Plasma Processes, 2020, vol. 24, no. 3, pp. 173–182. DOI: 10.1615/HighTempMatProc.2020035843.
22. Melnikov A.A., Shchur P.A. Transparent conductive antireflective coatings based on ITO, SiO2, TiO2. Trudy VIAM, 2019, No. 8 (80), paper no. 07. Available at: http://www.viam-works.ru (accessed: December 13, 2020). DOI: 10.18577 / 2307-6046-2019-0-8-56-66.
23. Rougier A. Nickel oxide based electrochromic materials. Materiaux pour l'énergie. Amiens, 2009, pp. 26–30.
24. Belousov A.L., Patrusheva T.N. Electrochromic oxide materials. Journal of the Siberian Federal University. Technics and techology, 2014, vol. 7, no. 6, pp. 698–709.
25. Wang J., Khoo E., Lee P.S., Ma J. Synthesis, assembly, and electrochromic properties of uniform crystalline WO3 nanorods. The Journal of Physical Chemistry C, 2008, vol. 112, no. 37, pp. 14306–14312.
26. Granqvist C.G. Electrochromic tungsten oxide films: review of progress 1993–1998. Solar Energy Materials and Solar Cells, 2000, vol. 60, no. 3, pp. 201–262.
27. Granqvist C.G. Handbook of Inorganic Electrochromic Materials, second impression. Elsevier, 2002, 650 p.
28. Dinh N.N., Oanh N.Th.T., Long P.D. et al. Electrochromic properties of TiO2 anatase thin films prepared by a dipping sol-gel method. Thin Solid Films, 2003, vol. 423, no. 1, pp. 70–76.
29. Ninh D.H., Thao T.T., Vo-Van T. Mixed nanostructured Ti–W oxides films for efficient electrochromic windows. Journal of Nanomaterials, 2012, vol. 2012, p. 7.
30. Handbook of inorganic electrochromic materials. Ed. C.G. Granqvist. Elsevier, 1995, 651 p.
31. Monk P.M.S., Mortimer R.J., Rosseinsky D.R. Electrochromism and electrochromic device. Cambridge: Cambridge University Press, 2007, 512 p.
32. Porqueras I., Person C., Corbella C., Vives M. Characteristics of e-beam deposited electrochromic CeO2 thin films. Solid State Ionics, 2003, vol. 165, no. 1-4, pp. 131–137.
33. Shchegolkov A.V., Chudov K.A. Obtaining thin, highly efficient electrochromic films based on nanostructured materials. Materials of All-Rus. Scientific Conf. “Technologies and materials for extreme conditions (predictive research and innovative development)”. Zvenigorod, 2018, pp. 66–70.
34. Shchegolkov A.V., Tugolukov E.N., Shchegolkov A.V. Overview of Electrochromic Materials and Devices: Scope and Development Prospects. Advanced Materials and Technologies, 2020, no. 2, pp. 66–73.
35. Vroon Z.A.E.P., Spee C.I.M.A. Sol-gel coatings on large area glass sheets for electrochromic devices. Journal of Non-Crystalline Solids, 1997, vol. 218, pp. 189–195.
36. Yanovskaya M.I., Obvintseva I.E., Kessler V.G. et al. Hydrolysis of molybdenum and tungsten alkoxides: sols, powders and films. Journal of Non-Crystalline Solids, 1990, vol. 124, no. 2-3, pp. 155–166.
37. Meda L., Breitkopf R.C., Haas T.E., Kirss R.U. Investigation of electrochromic properties of nanocrystalline tungsten oxide thin film. Thin Solid Films, 2002, vol. 402, no. 1-2, pp. 126–130.
38. Richardson T.J., Rubin M.D. Liquid phase deposition of electrochromic thin films. Electrochimica Acta, 2001, vol. 46, no. 13-14, pp. 2119–2123.
39. Nagayama H., Honda H., Kawahara H. A new process for silica coating. Electrochemical Society, 1988, vol. 135, pp. 2013–2016.
40. Zöller A., Götzelmann R., Matl K., Cushing, D. Temperature-stable bandpass filters deposited with plasma ion-assisted deposition. Applied Optics, 1996, vol. 35, no. 28, pp. 5609–5612.
41. Elinson V.M., Shchur P.A., Kirillov D.V. et al. Study of the Mechanical Characteristics of Single-Layer and Multilayer Nanostructures Based on Carbon and Fluorocarbon Coatings. Journal of Surface Investigation: X-ray, Synchrotron and Neutron Techniques, 2018, vol. 12, no. 2, pp. 357–360. DOI: 10.1134/S1027451018020246.
42. Elinson V.M., Shchur P.A., Deshevaya E.A., Kravets L.I. Antimicrobial antiadhesive properties of nanostructured fluorocarbon films obtained under transient conditions using two-component gas mixtures. Journal of Physics: Conference Series, 2019, vol. 1313, art. no. 012016. DOI: 10.1088/1742-6596/1313/1/012016.
43. Sleptsov V., Diteleva A. Thin-film technology for creating flexible supercapacitor electrodes based on a carbon matrix. High Temperature Material Processes: An International Quarterly of High-Technology Plasma Processes, 2020, vol. 24, no. 3, pp. 167–171
44. Macrelli G., Poli E. An all solid state inorganic thin film electrochromic device: device fabrication optical and electrochromical characterization. The Electrochemical Society Proceeding Series, 1996, vol. 5, no. 96-24, p. 338.
At present, the rapid development of aviation and aerospace technology imposes new requirements on materials for engine construction. to protect parts made of heat-resistant alloys from high-temperature gas corrosion, glass-based coatings are applied using a slip-firing technology. It is necessary to consider the possibility of improving such coatings by introducing modifying additives. As such additives, substances with sufficient chemical and thermal resistance should be considered. As a rule, these are compounds of silicon, boron, rare and rare earth metals. Metal silicides are known for their ability to resist oxidation in an oxygen environment up to 1500 °C. The most well-studied is molybdenum disilicide (MoSi2). In addition, the introduction of more refractory tungsten in the composition along with molybdenum allows you to control such important properties as: the coefficient of thermal expansion, the characteristics of corrosion resistance at different temperatures, mechanical properties, etc. Zirconium, hafnium, and silicon borides are also widely used. Their use allows you to reduce the temperature of the coating formation, reduces the surface roughness, creates the effect of self-healing cracks. lanthanum compounds are characterized by high temperature and chemical resistance, low porosity. the most well-known glass-ceramic materials based on chromites and lanthanum aluminates. Also noteworthy are rare earth metal zirconates and hafnates that have a pyrochlore structure (for example, La2Zr2O7), since they are thermally stable up to the melting point (about 2300 °C) and have extremely low thermal conductivity and high corrosion resistance. Fluorites (for example, La2Ce2O7), perovskites (for example, SrZrO3), and complex spinels (for example, LaMgAl11O19) are considered equally promising materials. when th
2. Ospennikova O.G., Podieiachev V.N., Stoliankov Yu.V. Refractory alloys for innovative equipment. Trudy VIAM, 2016, no. 10, paper no. 5. Available at: http://www.viam-works.ru (accessed: November 18, 2020). DOI: 10.18577/2307-6046-2016-0-10-5-5.
3. Kablov E.N., Solntsev S.S., Rosenenkova V.A., Mironova N.A. Modern polyfunctional high-temperature coatings for nickel alloys, sealing metal materials and beryllium alloys. Novosti materialovedeniya. Nauka i tekhnika, 2013, no. 1, paper no. 05. Available at: http://www.materialsnews.ru (date accessed: November 23, 2020).
4. Grashchenkov D.V. Strategy of development of non-metallic materials, metal composite materials and heat-shielding. Aviacionnye materialy i tehnologii, 2017, no. S, pp. 264–271. DOI: 10.18577/2071-9140-2017-0-S-264-271.
5. Kablov E.N., Grashchenkov D.V., Isaeva N.V., Solntsev S.S. Promising high-temperature ceramic composite materials. Rossiyskiy khimicheskiy zhurnal, 2010., vol. LIV, no. 1, pp. 20–24.
6. Kablov E.N., Grashchenkov D.V., Isaeva N.V., Solntsev S.S., Sevastianov V.G. High-temperature structural composite materials based on glass and ceramics for advanced aircraft products. Steklo i keramika, 2012, no. 4, pp. 7–11.
7. Zhitnyuk S.V. Oxygen-free ceramic mate-rials for the space technics (review). Trudy VIAM, 2018, no. 8 (68), paper no. 08. Available at: http://www.viam-works.ru (accessed: November 11, 2020). DOI: 10.18577/2307-6046-2018-0-8-81-88.
8. Wang G., Jiang W., Bai G., Wu Li. Effect of Addition of Oxides on Low-Temperature Oxidation of Molybdenum Disilicide. Journal of American Ceramic Society, 2003, vol. 86, no. 4, pp. 731–734.
9. Titov D.D., Kargin Yu.F., Popov N.A., Lysenkov A.S. New composite materials based on molybdenum disilicide. Perspektivnye materialy, 2011, no. S13, pp. 493–499.
10. Han X., Wang Y.-L., Xiong X., Li H. Microstructure, sintering behavior and mechanical properties of SiC / MoSi2 composites by spark plasma sintering. Transaction of Nonferrous Metals Sosiety of Chaina, 2018, no. 28, pp. 957–965. DOI: 10.1016/S1003-6326 (18) 64730-2.
11. Gnesin I.B. Experimental study of the structure and properties of solid solutions of molybdenum and tungsten silicides and their application: thesis, Cand. Sc. (Tech.). Chernogolovka: Institute of Solid State Physics RAS, 2005, 24 p.
12. Gnesin I.B., Gnesin B.A., Nekrasov A.N. Investigation of the effect of carbon impurity on microhardness, chemical and phase compositions of double silicide eutectics Me5Si3–MeSi2 of the Mo–W–Si system on cast samples. Materialovedenie, 2008, no. 8, pp. 21–35.
13. Armor for «Buran». Materials and technologies of VIAM for the ISS «Energiya–Buran». Ed. E.N. Kablov. Moscow: Nauka i zhizn, 2013, 128 p.
14. Kablov E.N. Materials for «Buran» spaceship – innovative solutions of formation of the sixth technological mode. Aviacionnye materialy i tehnologii, 2013, no. S1, pp. 3–9.
15. Kablov E.N., Solntsev S.S. Oxythermosynthesis – a new step towards materials for advanced aerospace technology. Aviation materials. Selected works of VIAM 1932–2002. Moscow: VIAM, 2002, pp. 131–137.
16. Goldstein H.E., Leiser D.B., Katvala V. Reaction cured borosilicate glass coating for low density fibrous silica insulation. Borate Glasses. Materials science research: plenum press. New York; London, 1978, vol. 12, pp. 623–634.
17. Goldstein N.V. et al. Reaction cured borosilicate glass coating for low-density fibrous insulation. Borate glasses. Structure, properties, application: plenum press. New York, 1978, pp. 623–634.
18. Garofalini S.H., Banas R., Creedon J. Development of high viscosity coatings for advances Space Shuttle application. 11th National SAMPE technical conference. Boston, 1979, pp. 114–124.
19. Stratiychuk D.A. Impregnation of amorphous boron with silicon melt under conditions of high pressures and temperatures. Dopovidi Nacionalnoi akademii nauk Ukraini, 2011, no. 3, pp. 94–99.
20. Matsushita J., Komarneni S. High temperature oxidation of silicon hexaboride ceramics. Materials Research Bulletin, 2001, vol. 36, no. 5-6, pp. 1083–1089.
21. Tong Ch., Cheng L., Yin X. et al. Oxidation behavior of 2D C/SiC composite modified by SiB4 particles in inter-bundle pores. Composites Science and Technology, 2008, vol. 68, pp. 602–607.
22. Pryamilova E.N., Lyamin Yu.B. Ultra-high-temperature ceramics based on borides. Collection of materials of the V Internat. conf. with elements of scientific schools for young people «Functional nanomaterials and high-purity substances». Suzdal, 2014, pp. 447–448.
23. Pryamilova E.N., Poilov V.Z., Lyamin Yu.B. Thermochemical stability of ceramics based on zirconium and hafnium borides. Vestnik Permskogo natsionalnogo issledovatelskogo politekhnicheskogo universiteta, 2014, no. 4, pp. 55–67.
24. Mazilin I.V., Baldaev L.Kh., Drobot D.V., Akhmetgareeva A.M., Zhukov A.O., Khismatullin A.G. Thermal and thermophysical properties of heat-protective coatings based on lanthanum zirconate. Perspektivnye materialy, 2013, no. 7, pp. 21–30.
25. Merkushkin A.O., Zaw Ye Maw Oo. Obtaining and properties of ceramics from lanthanum and gadolinium aluminates. Scientific Researches and Their Practical Application, 2012, vol. 32, no. 3, pp. 8–9.
26. Stefanovskiy S.V., Stefanovskaya O.I., Semenova D.V. Phase composition and structure of sodium-aluminum phosphate-based glass materials containing oxides of rare-earth elements. Radioaktivnye otkhody, 2018, no. 1 (2), pp. 97–101.
27. Galasso F.S. Structure, properties and preparation of perovskite-type compounds. Oxford: Pergamon Press, 1969, 209 p.
28. Vitkalova I.A., Torlova A.S., Pikalov E.S. Influence of lanthanum oxide on the properties of chemically resistant ceramics obtained using galvanic sludge. Mezhdunarodnyy nauchno-issledovatelskiy zhurnal, ser.: Technical sciences, 2019, no. 10, pp. 35–39. DOI: 10.23670/IRJ.2019/88/10/006.
29. Dudkin B.N., Bugaeva A.Yu., Zainullin G.G. Features of sintering xerogel of the composition «lanthanum hexaaluminate – yttrium oxide» obtained by the sol-gel method. Izvestiya Komi nauchnogo tsentra UrO RAN, 2011, no. 2, pp. 19–24.
30. Pyachin A.S., Ershova T.B., Burkov A.A., Vlasova N.M., Komarova V.S. The use of titanium aluminides for the creation of electrospark coatings. Poroshkovaya metallurgiya i funktsional'nyye pokrytiya. Izvestiya vuzov, 2015, no. 1, pp. 55–61.
31. Karashaev M.M., Lomberg B.S., Bakradze M.M., Letnikov M.N. On technological approaches to the creation of composite materials based on nickel monoaluminide NiAl (review). Trudy VIAM, 2019, no. 12 (84), paper no. 07. Available at: http://www.viam-works.ru (accessed: December 18, 2020). DOI: 10.18577/2307-6046-2019-0-12-55-66.
32. Bankovskaya N.V. Creation of a new generation of high-temperature glass-ceramic compositions and study of their physical and chemical properties: thesis, Dr. Sc. (Chem.). Saint Petersburg: Order of the Red Banner of Labor Institute of silicates named after I.V. Grebenshchikov Russian Academy of Sciences, 2006, 297 p.
33. Vasenev V.V. Development of composite materials based on Al–Si–Ni systems with low thermal expansion coefficient and technology for producing semi-finished products for rocket and space technology: thesis, Cand. Sc. (Tech.). Moscow: Moscow Institute of Aviation Materials, 2017, 135 p.
In this article the changes in the microstructure and phase composition of Zr–Y – based alloy (VTsM-1) samples for the manufacture of magnetron targets are discussed; it is used two different technologies for Zr–Y magnetron target manufacturing: on the basis of vacuum induction melting and on the basis of vacuum arc melting.
It has been shown that a switch in the manufacturing technology of VTsM-1 alloy – from the basis on vacuum induction melting to the basis on vacuum arc melting leads to the resulting changes:
a) the concentration of interstitial impurities, such us oxygen, in the Zr–Y alloy, from 3–4% to 1–2% (according to the X-Ray spectral microanalysis data).
b) the content of the α-Y-based phase on in the alloy were increased from 5–10% to 15–30%;
c) the a and c crystal lattice periods of the hexagonal phases were increased: both the main phase – α-Zr-based solid solution, and α-Y-based second phase – from the initial to the increased on 0.01–0.02 nm; the а crystal lattice period of the cubical phase (α-Y2O3 oxide) also was increased to 0.001 nm from initial.
c) there is a change in the nature of the distribution of particles of the second phase based on the α-Y solid solution in the microstructure of the Zr–Y alloy – from a similar dispersed particle distribution in the volume of the alloy – to the concentration of this phase along the grain boundaries.
2. Kablov E.N., Muboyadzhyan S.A., Budinovskiy S.A., Pomelov Ya.A. Ion-plasma protective coatings for blades of gas turbine engines. Konversiya v mashinostroyenii, 1999, no. 2, pp. 42–47.
3. Sokolov A.V., Deynega G.I., Kuzmina N.A. Influence of Sc2O3 additive on sintering tempera-ture and properties of ZrO2–Y2O3 system oxide ceramics. Aviacionnye materialy i tehnologii, 2020, no. 1 (58), pp. 64–69. DOI: 10.18577/2071-9140-2020-0-1-64-69.
4. Loshchinin Yu.V., Budinovskiy S.A., Razmakhov M.G. Heat conductivity of heat-protective coatings ZrO2–Y2O3 alloyed by REM oxides obtained by magnetronny application. Aviaсionnye materialy i tehnologii, 2018, no. 3, pp.42–49. DOI: 10.18577/2071-9140-2018-0-3-42-49.
5. Kablov E.N., Muboyadzhyan S.A., Budinovskiy S.A., Lutsenko A.N. Ion-plasma protective coatings for blades of gas turbine engines. Metally, 2007, no. 5, pp. 23–34.
6. Kablov E.N., Muboyadzhyan S.A. Heat resisting and heat-protective coverings for turbine blades of high pressure of perspective GTE. Aviacionnye materialy i tehnologii, 2012, no. S, pp. 60–70.
7. Aleksandrov D.A., Muboyadzhyan S.A., Zhuravleva P.L., Gorlov D.S. Investigation of the effect of surface preparation and ion-assisted deposition on the structure and properties of erosion-resistant ion-plasma coating. Trudy VIAM, 2018, no. 10 (70), paper no. 08. Available at: http://www.viam-works.ru (accessed: December 01, 2020). DOI: 10.18577/2307-6046-2018-0-10-62-73.
8. Budinovsky S.A., Stekhov P.A., Doronin O.N., Artemenko N.I. Main mechanisms of destruction of the ceramic layer of thermal barrier coatings (review). Trudy VIAM, 2019, no. 2 (74), paper no. 11. Available at: http://www.viam-works.ru (accessed: August 11, 2020). DOI: 10.18577 / 2307-6046-2019-0-2-105-112. (accessed: December 01, 2020). DOI: 10.18577 / 2307-6046-2019-0-2-105-112.
9. Valyukhov S.G., Stogney O.V., Filatov M.S. Influence of magnetron sputtering conditions on the structure of heat-resistant nanostructured coatings made of zirconium dioxide ZrO2. Izvestiya vysshikh uchebnykh zavedeniy. Mashinostroyeniye, 2015, no. 11 (668), pp. 97–105. DOI: 10.18698/0536-1044-2015-11-97-105.
10. Sergeev V.P., Neifeld V.V., Sungatulin A.R., Sergeev O.V., Fedorishcheva M.V., Nikalin A.Yu. Increase in thermal cycling resistance of coatings based on Zr–Y–O obtained by magnetron deposition. Izvestiya Tomskogo politekhnicheskogo universiteta, 2010, vol. 317, no. 2, pp. 111–115.
11. Budinovsky S.A., Kablov E.N., Muboyadzhyan S.A., Novikov V.N., Pomelov A.Ya. High-energy vacuum plasma technology – an effective way to create new coatings and materials. Aviation materials at the turn of the XX–XXI centuries. Moscow: VIAM, 1994, pp. 314–325.
12. Kablov E.N., Muboyadzhyan S.A., Budinovskiy S.A., Galoyan A.G., Lutsenko A.N. Protective and hardening coatings of blades and gas turbine engine parts. 75 years. Aviation materials. Moscow: VIAM, 2007, pp 107–124.
13. Kablov E.N., Muboyadzhyan S.A. Heat-protective coatings with a ceramic layer of low thermal conductivity based on zirconium oxide for high-pressure turbine blades of promising gas turbine engines. Reports of conf. "Modern achievements in the field of creating promising non-metallic composite materials and coatings for aviation and space technology". Moscow: VIAM, 2015, p. 3.
14. Muboyadzhyan S.A., Kablov E.N., Budinovskiy S.A. Vacuum-plasma technology for producing protective coatings from complex alloyed alloys. Metallovedenie i termicheskaya obrabotka metallov, 1995, no. 2, pp. 15–18.
15. Bu M.J., Wang P.S., Xu H.H. et al. Experimental Investigation and Thermodynamic Modeling of the Zr–Y System. Journal of Mining and Metallurgy, section B: Metallurgy, 2010. Vol. 46 (2). P. 181–192. DOI: 10.2298/JMMB1002181B.
16. Abriata J.P., Garcés J., Versaci R. The O-Zr (Oxygen-Zirconium) System. Bulletin of Alloy Phase Diagrams. 1986. Vol. 7, no. 2. P. 116–124.
17. Okamoto H. O–Y (Oxygen–Yttrium). Journal of Phase Equilibria and Diffusion, 2011, vol. 32, no. 6, p. 574. DOI: 10.1007/s11669-011-9956-0.
18. Bronfin M.B., Alekseev A.A., Chabina E.B. Metallophysical research: opportunities and prospects. 75 years. Aviation materials. Moscow: VIAM, 2007, 353–365.
19. Gorelik S.S., Skakov Yu.A., Rastorguev L.N. X-ray and electron-optical analysis: textbook. Moscow: MISIS, 2002, 360 p.
20. Umansky Ya.S., Skakov Yu.A., Ivanov A.N., Rastorguev L.N. Crystallography, X-ray and electron microscopy. Moscow: Metallurgiya, 1982, 632 p.
The issues of PCM aging in natural conditions in various climatic zones are given great attention by both domestic and foreign scientists. It is noted that climatic factors have a significant impact on the PCM during long-term operation of products: temperature, relative factors negatively affect the strength characteristics of materials, which in turn reduces the resource of structures made with their use. To predict the service life of structures made with the use of PCM, it is necessary to study the resistance of materials to the effects of climatic factors mentioned above.
This article presents the results of studies of the properties of carbon fiber vku-51 and fiberglass vps-58 based on epoxivinyl ether binder, intended for the manufacture of load-bearing building structures of bridge structures, after a long exposure (for 5 years with intermediate removals after 1 year and 3 years) These materials Are used in different climatic zones. The exhibition included plates with dimensions of 300×300 mm and a thickness of 2.5 mm (carbon fiber) and 3.5 mm (fiberglass) without applying a protective paint coating.
When assessing the appearance of the exposed PCM plates, it can be stated that the degradation of the surface of materials is observed after 1 year of exposure, which is not critical, because even after 5 years of exposure, the preservation of properties is quite high.
VKU-51 carbon fiber and VPS-58 fiberglass showed a high level of preservation of physical and mechanical properties after prolonged exposure to operational factors (70–100% depending on the type of test), which indicates resistance to external influences in various climatic zones. At The same time, it should be noted that the most aggressive impact on carbon fiber has the industrial atmosphere of moscow. The most aggressive impact on fiberglass&
2. On national goals and strategic objectives of the development of the Russian Federation for the period until 2024: Decree of the President of the Russian Federation No. 204 (May 07, 2018). Available at: http://www.kremlin.ru/acts/bank/43027 (accessed: December 07, 2020).
3. National Program for the Development of the Far East: Order of the Government of the Russian Federation No. 2464-р (September 24, 2020). Available at: http://www.government.ru/docs/40487 (accessed: December 07, 2020).
4. Kablov E.N. VIAM: new generation materials for PD-14. Krylya Rodiny, 2019, no. 7-8, pp. 54–58.
5. Mishkin S.I., Raskutin A.E., Evdokimov A.A., Gulyaev I.N. Technologies and the main stages of construction of the arch bridge first in Russia from composite materials. Trudy VIAM, 2017, no. 6 (54), paper no. 05. Available at: http://www.viam-works.ru (accessed: December 10, 2020). DOI: 10.18577/2307-6046-2017-0-6-5-5.
6. Evdokimov A.A., Raskutin A.E., Mishkin S.I., Mikhaldykin E.S. Arched bridges with the use of carbon-fiber arched elements. Konstruktsii iz kompozitsionnykh materialov, 2019, no. 2 (154), pp. 22-29.
7. Gladkikh A.V., Kurs I.S., Kurs M.G. Analysis of the data of full-scale climatic tests combined with the application of operational factors of nonmetallic materials (review). Trudy VIAM, 2018, no. 10 (70), paper no. 09. Available at: http://www.viam-works.ru (accessed: December 06, 2020). DOI: 10.18577/2307-6046-2018-0-10-74-82.
8. Kablov E.N., Kirillov V.N., Zhirnov A.D., Startsev O.V., Vapirov Yu.M. Centers for climatic testing of aviation PCM. Aviatsionnaya promyshlennost, 2009, no. 4, pp. 36–46.
9. Kablov E.N., Startsev O.V. The basic and applied research in the field of corrosion and ageing of materials in natural environments (review). Aviacionnye materialy i tehnologii, 2015, no. 4 (37), pp. 38–52. DOI: 10.18577/2071-9140-2015-0-4-38-52.
10. Kablov E.N., Startsev V.O. Systematical analysis of the climatics influence on mechanical properties of the polymer composite materials based on domestic and foreign sources (review). Aviacionnye materialy i tehnologii, 2018, no. 2 (51), pp. 47–58. DOI: 10.18577/2071-9140-2018-0-2-47-58.
11. Aviation materials: reference book in 13 vols. Ed. E.N. Kablov. 7th ed., rev. and add. Moscow: VIAM, 2015, vol. 13: Climatic and microbiological resistance of non-metallic materials, 270 p.
12. Kablov E.N., Startsev V.O., Inozemtsev A.A. The moisture absorption of structurally similar samples from polymer composite materials in open climatic conditions with application of thermal spikes. Aviacionnye materialy i tehnologii, 2017, no. 2 (47), pp. 56–68. DOI: 10.18577/2071-9140-2017-0-2-56-68.
13. Laptev A.B., Barbotko S.L., Nikolaev E.V. The main research areas of the persistence properties of materials under the influence of climatic and operational factors. Aviacionnye materialy i tehnologii, 2017, no. S, pp. 547–561. DOI: 10.18577/2071-9140-2017-0-S-547-561.
14. Roylance D., Roylance M. Weathering of fiber-reinforced epoxy composites. Polymer Engineering and Science, 1978, vol. 18, no. 4, pp. 249–254.
15. Belec L., Nguyen T.H., Nguyen D.L., Chailan J.F. Comparative effects of humid tropical weathe-ring and artificial ageing on a model composite properties from nano- to macro-scale. Composites, part A, 2015, vol. 68, no. 1, pp. 235–241.
16. De Bruijn J.C.M., Meijer H.D.F. The design and application of a microfoil tensile test apparatus for monitoring the degree of ultraviolet degradation of polymers. Review of Scientific Instruments, 1991, no. 62, pp. 1620–1623.
17. De Bruijn J.C.M. Degradation profiles of thick high-density polyethylene samples after outdoor and artificial weathering. Polymer durability: degradation, stabilization, and lifetime prediction. Washington: American Chemical Society, 1996, pp. 599–620.
18. Gu X., Dickens B., Stanley D. et al. Linking accelerating laboratory test with outdoor performance results for a model epoxy coating system. Iowa State University, 2008, pp. 1–47.
19. Deev I.S., Kuryshev E.V., Lonsky S.L., Zhelezina G.F. Influence of long-term climatic aging on the surface microstructure of epoxy organoplastics and the nature of its destruction under bending conditions. Voprosy materialovedeniya, 2016, no. 3 (87), pp. 104-114.
20. Startsev V.O. Climatic resistance of polymer composite materials and protective coatings in moderately warm climates: thesis, Dr. Sc. (Tech.). Moscow: VIAM, 2018, 308 p.
21. Startsev V.O., Valevin E.O., Gulyaev A.I. The influence of polymer composite materials’ surface weathering on its mechanical properties. Trudy VIAM, 2020, no. 8 (90), paper no. 07. Available at: http://www.viam-works.ru (accessed: December 11, 2020). DOI: 10.18577/2307-6046-2020-0-8-64-76.
|
Authors named |
Position, academic degree |
Affiliation |
|
Leonid Yu. Avilochev |
Leading Engineer |
FSUE «All-Russian scientific research institute of aviation materials» SSC of RF; e-mail: This email address is being protected from spambots. You need JavaScript enabled to view it. |
|
Anna yu. Anisimova |
Engineer |
|
|
Anton I. Vasilev |
Technician |
|
|
Elena M. Visik |
Head of Sector, Candidate of Sciences (Tech.) |
|
|
Vitaliy A. Goncharov |
Head of Laboratory |
|
|
Liliya N. Grigoreva |
Engineer |
|
|
Ivan N. Gulyaev |
Deputy Head of Laboratory for Science, Candidate of Sciences (Tech.) |
|
|
Valentina S. Denisova |
Head of Sector |
|
|
Anton A. Evdokimov |
Engineer |
|
|
Evgeny S. Elyutin |
Leading Engineer |
|
|
Viktor I. Ivanov |
Leading Researcher |
|
|
Alexey Yu. Isaev |
Head of Laboratory, Candidate of Sciences (Tech.) |
|
|
Stanislav V. Kondrashov |
Deputy Head of Laboratory for Science, Doctor of Sciences (Tech.) |
|
|
Elena V. Kotova |
Leading Engineer |
|
|
Elena I. Kurbatkina |
Head of Laboratory, Candidate of Sciences (Tech.) |
|
|
Sergey A. Larionov |
Engineer First Category |
|
|
Galina A. Malinina |
Engineer Second Category, Candidate of Sciences (Chem.) |
|
|
Nadezhda A. Nochovnaya |
Deputy Head of Laboratory, Doctor of Sciences (Tech.) |
|
|
Andrey N. Nyafkin |
Head of Sector |
|
|
Roman M. Nazarkin |
Leading Engineer |
|
|
Konstantin A. Pavlovskiy |
Deputy Head of Laboratory |
|
|
Aleftina P. Petrova |
Chief Researcher, Doctor of Sciences (Tech.) |
|
|
Nikolay V. Petrushin |
Chief Researcher, Doctor of Sciences (Tech.) |
|
|
Alexander V. Platitsin |
Leading Engineer, Candidate of Sciences (Tech.) |
|
|
Stanislav V. Putyrskiy |
Deputy Head of Laboratory |
|
|
Alexander A. Pykhtin |
Deputy Head of Laboratory, Candidate of Sciences (Tech.) |
|
|
Ekaterina V. Rubtsova |
Head of Sector |
|
|
Valeria A. Sagomonova |
Head of Laboratory |
|
|
Viktoria M. Serpova |
Leading Engineer |
|
|
Denis V. Sidorov |
Leading Researcher, Candidate of Sciences (Tech.) |
|
|
Stanislav S. Solntsev |
Counselor of Director General, Doctor of Sciences (Tech.) |
|
|
Lyudmila V. Solovyanchik |
Head of Sector |
|
|
Anton E. Sorokin |
Head of Scientific-Research Bureau, Candidate of Sciences (Tech.) |
|
|
Maxim N. Sutyagin |
Second Category Engineer |
|
|
Pavel N. Timoshkov |
Head of Scientific-Research Bureau |
|
|
Maria N. Usacheva |
Second Category Technician |
|
|
Alexandr V. Hrulkov |
Leading Engineer-technologist |
|
|
Elena B. Chabina |
Leading Researcher, Candidate of Sciences (Tech.) |
|
|
Pavel A. Shchur |
Junior Researcher |
FSBEI of HPE «Moscow Aviation Institute (National Research University)»; e-mail: This email address is being protected from spambots. You need JavaScript enabled to view it. |
|
Andrey Yu. Korotchenko |
Head of a Chair, Doctor of Sciences (Tech.) |