Firmness of paint coatings at influence of gas-abrasive and gas-droplet erosion

Kuznetsova V.A., Marchenko S.A., Zheleznyak V.G., Kovrizhkina N.A.
Kuznetsova V.A., Marchenko S.A., Zheleznyak V.G., Kovrizhkina N.A. Firmness of paint coatings at influence of gas-abrasive and gas-droplet erosion // Proceedings of VIAM. 2024. No. 4. DOI: 10.18577/2307-6046-2024-0-4-133-144. URL: https://www.viam-works.ru/en/journal/2024/4/10
Keywords
gas-abrasive erosion, gas-droplet erosion, erosion depth, adhesive durability, durability at stretching, erosion resistance, systems of paint coatings
Abstract

The analysis of test results on stability to gas-abrasive erosion for systems of paint coatings based on the erosion-resistant disperse-reinforced enamel EP-5236 applied on aluminum alloy D16-T and fibreglass VPS-20 at impact angles α = 90° and 15° was carried out. Firmness of coatings was evaluated on changes of weight characteristics of samples. Resistance of paint coatings to gas-droplet erosion on samples from alloy D16-T and also from fibreglass VPS-20 was investigated. It is shown that using of erosion-resistant system of paint coatings based on disperse-reinforced enamel EP-5236 increases resistance to gas-abrasive and gasdroplet erosion

Reference list
  1. Kablov E.N. Aviation materials science: results and prospects. Vestnik Rossiyskoy akademii nauk, 2002, vol. 72, no. 1, pp. 3–12.
  2. Kablov E.N. The role of chemistry in the creation of new generation materials for complex technical systems. Report XX Mendeleev Congress on General and Applied Chemistry: in 5 vols. Ekaterinburg: Ural Branch of the Russian Academy of Sciences, 2016, vol. 1: Fundamental problems of chemical science, pp. 25–26.
  3. Startsev V.O., Antipov V.V., Slavin A.V., Gorbovets M.A. Modern domestic polymer composite materials for aviation industry (review). Aviation materials and technologies, 2023, no. 2 (71), paper no. 10. Available at: http://www.journal.viam.ru (accessed: February 07, 2024). DOI: 10.18577/2713-0193-2023-0-2-122-144.
  4. Kuznetsova V.A., Shapovalov G.G. Tendencies of development of the erosion-resistant coatings (review). Trudy VIAM, 2018, no. 11 (71), paper no. 09. Available at: http://www.viam-works.ru (accessed: February 07, 2024). DOI: 10.18577/2307-6046-2018-0-11-74-85.
  5. Pavlyuk B.Ph. The main directions in the field of development of polymeric functional materials. Aviacionnye materialy i tehnologii, 2017, no. S, pp. 388–392. DOI: 10.18577/2071-9140-2017-0-S-388-392.
  6. Erosion. Ed. K. Preece; trans. from Engl. Moscow: Mir, 1982, 464 p.
  7. Perelman R.G. Erosion strength of aircraft engine parts and power plants. Moscow: Mashinostroyenie, 1980, 246 p.
  8. Khrushchov M.M., Babichev M.A. Abrasive wear. Moscow: Nauka, 1970, 252 p.
  9. Urvantsov L.A. Erosion and protection of metals. Moscow: Mashinostroyenie, 1966, 235 p.
  10. Springer J. Erosion under the influence of liquid drops. Moscow: Mashinostroyenie, 1981, 200 p.
  11. Nepomnyashchiy E.F. Contact interaction of solids and calculation of friction and wear forces. Moscow: Nauka, 1971, 270 p.
  12. Zhelezina G.F., Solovieva N.A., Kulagina G.S., Shuldeshova P.M. Study of the possibility of increasing the impact resistance of thin-sheeted carbon fiber-reinforced plastics due to clading with aramid organoplastics. Aviation materials and technologies, 2021, no. 4 (65), paper no. 04. Available at: http://www.journal.viam.ru (accessed: February 07, 2024). DOI: 10.18577/2713-0193-2021-0-4-35-42.
  13. Kondrashov E.K., Lebedeva T.A. Erosion-resistant coatings for the protection of polymer composite materials. Aviacionnye materialy i tehnologii, 2003, is.: Paints and varnishes and coatings, pp. 57–58.
  14. Kondrashov E.K., Naidenov N.D. Erosion resistant paint coverings of aviation purpose. Part 1. Erosion resistant paint coatings based on epoxy and polyurethane films forming (review). Trudy VIAM, 2020, no. 2 (86), paper no. 09. Available at: http://www.viam-works.ru (accessed: February 07, 2024). DOI: 10.18577/2307-6046-2020-0-2-81-90.
  15. Kondrashov E.K., Naidenov N.D. Erosion-resistant paint and varnish coatings for aviation purposes. Part 2. Elastomeric erosion resistant radio-transparent coatings (review). Trudy VIAM, 2020, no. 3 (87), paper no. 10. Available at: http://www.viam-works.ru (accessed: January 29, 2024). DOI: 10.18577/2307-6046-2020-0-3-94-101.
  16. Kuznetsova V.A. Erosion-resistant composition based on the three-phase system «epoxy oligomer–rubber–reinforcing filler»: thesis abstract, Cand. Sc. (Tech.). Moscow, 1999, 24 p.
  17. Merkulova Yu.I., Kurshev E.V., Vdovin A.I., Andreeva N.P. Microstructural and electrochemical studies of paint coatings under natural climate tests of tropical climate of North America. Aviation materials and technologies, 2022, no. 2 (67), paper no. 11. Available at: http://www.journal.viam.ru (accessed: February 07, 2024). DOI: 10.18577/2713-0193-2022-0-2-120-130.
  18. Kozlova A.A., Kondrashov E.K. Influence of molecular weight and elemental composition of isocyanates on the properties of fluoropolyurethane enamels. Aviation materials and technologies, 2023, no. 4 (73), paper no. 09. Available at: http://www.journal.viam.ru (accessed: February 07, 2024). DOI: 10.18577/2713-0193-2023-0-4-92-100.
  19. Kuznetsova V.А. Influence of the elastomeric modifier on mechanical and viscoelastic properties of epoxy and rubber compositions for erosion resistant coatings. Aviacionnye materialy i tehnologii, 2020, no. 2 (59), pp. 56–62. DOI: 10.18577/2071-9140-2020-0-2-56-62.
  20. Berlin A.A., Basin V.E. Basics of polymer adhesion. Moscow: Khimiya, 1969, 318 p.
  21. Kovrizhkina N.A., Kuznetsova V.A., Silaeva A.A., Marchenko S.A. Ways to improve the properties of paint coatings by adding different fillers (review). Aviacionnye materialy i tehnologii, 2019, no. 4 (57), pp. 41–48. DOI: 10.18577/2071-9140-2019-0-4-41-48.
  22. Silaeva A.A., Kuznetsova V.A., Kurshev E.V., Timoshina E.A. Influence of the dimensions of the reinforcing filler on the technological and functional properties of paints and varnishes. Materialovedenie, 2022, no. 2, pp. 32–38.
  23. Zheleznyak V.G., Serdcelyubova A.S., Merkulova Yu.I., Skivko P.V. Paint coating system based on polyurethane enamel for protecting heated frontal surfaces of aviation products. Aviation materials and technologies, 2022, no. 1 (66), paper no. 10. Available at: http://www.journal.viam.ru (ассеssed: February 07, 2024). DOI: 10.18577/2713-0193-2022-0-1-120-128.
  24. Goldberg M.M., Koryukin A.V., Kondrashov E.K. Coatings for polymer materials. Moscow: Khimiya, 1980, 287 p.
  25. Vladimirsky V.N., Denker I.I., Chebotarevsky V.V. Installation for determining the erosion resistance of polymer coatings. Lakokrasochnye materialy i ikh primenenie, 1973, no. 1, pp. 54–56.
  26. Kashcheev V.N. Abrasive wear of solids. Moscow: Nauka, 1970, 248 p.
  27. Nepomnyashchiy E.F. Contact interaction of solids and calculation of friction and wear forces. Moscow: Nauka, 1971, 240 p.
  28. Chernoyarov S.A., Ivanov A.V., Borkova A.N., Pomakhaeva L.I., Pomakhaev V.P., Kovalev I.E. Installation of a centrifugal self-balancing type TsS-871 and methods of testing materials for resistance to droplet impact erosion. Aviacionnye materialy i tehnologii, 2003, no. 3, pp. 68–72.
  29. Kondrashov E.K. Paints and varnishes and coatings based on them in mechanical engineering. Moscow: Paint-Media, 2021, 255 p.
  30. Chernoyarov S.A., Ivanov A.V., Borkova A.N., Pomakhaeva L.I., Pomakhaev V.P., Ani-khovskaya L.I., Kuznetsova V.A. Study of resistance to drop impact erosion of fiberglass laminate with polymer protective coatings. Aviacionnye materialy i tehnologii, 2003, no. 3, pp. 73–75.
  31. Erasov V.S., Kotova E.A. Erosion resistance of aviation materials to influence of solid (dust) particles. Aviacionnye materialy i tehnologii, 2011, no. 3, pp. 30–36.
  32. Kramchenkov E.M. Study of erosive wear of materials: thesis abstract, Cand. Sci. (Tech.). Moscow, 1996, 26 p.
  33. Borkova A.N. Erosion resistance of aviation materials upon impact with solid (dust) particles: thesis abstract, Cand. Sci. (Tech.). Moscow, 2006, 27 p.
  34. Alekseev V.K., Bodryshev V.V., Nozhnitsky Yu.A. Some features of destruction and wear of materials during interaction with solid and liquid particles. Trenie i iznos, 1981, vol. 1. no. 2, рр. 239–246.
  35. Kleis I.R. Fundamentals of material selection when working under conditions of gas abrasive wear. Trenie i iznos, 1980, vol. 1, no. 2, pp. 263–274.
  36. Kablov E.N. Innovative developments of FSUE «VIAM» SSC of RF on realization of «Strategic directions of the development of materials and technologies of their processing for the period until 2030». Aviacionnye materialy i tehnologii, 2015, no. 1 (34), pp. 3–33. DOI: 10.18577/2071-9140-2015-0-1-3-33.