Analysis of molybdenum by high resolution glow discharge mass spectrometry
UDC
543.51:669.1
DOI
10.18577/2307-6046-2024-0-2-92-101
Article PDF (Russian)
(701.4 KB)
How to cite
Alekseev A.V., Yakimovitch P.V. Analysis of molybdenum by high resolution glow discharge mass spectrometry // Proceedings of VIAM. 2024. No. 2. DOI: 10.18577/2307-6046-2024-0-2-92-101. URL: https://www.viam-works.ru/en/journal/2024/2/10
Keywords
high resolution glow discharge mass spectrometry, molybdenum, molybdenum alloys, determination of harmful impurities
Abstract
In this work, we determined the impurities of 43 elements in molybdenum using high-resolution glow discharge mass spectrometry. Sample preparation for analysis is described. To achieve maximum analytical signals from all the required elements, the appropriate equipment settings have been selected. Spectral interferences are eliminated due to the use of high resolution. The relative sensitivity coefficients were calculated for all determined elements using the X-ray fluorescence spectroscopy method.
Reference list
- Kablov E.N. The strategic directions of development of materials and technologies of their processing for the period to 2030. Aviacionnye materialy i tehnologii, 2012, no. S, pp. 7–17.
- Min P.G., Vadeev V.E., Kramer V.V. The development of the new VZhM200 superalloy and the technology of its production for casting of the advanced engines’ blades by the directional crystallization. Aviation materials and technologies, 2021, no. 3 (64), paper no. 02. Available at: http://www.journal.viam.ru (accessed: December 04, 2023). DOI: 10.18577/2071-9140-2021-0-3-11-18.
- Kablov E.N., Echin A.B., Bondarenko Yu.A. History of development of directional crystallization technology and equipment for casting blades of gas turbine engines. Trudy VIAM, 2020, no. 3 (87), paper no. 01. Available at: http://www.viam-works.ru (accessed: December 04, 2023). DOI: 10.18577/2307-6046-2020-0-3-3-12.
- Svetlov I.L., Petrushin N.V., Epishin A.I., Kara-shaew M.M., Elyutin E.S. Single crystals of nickel-based superalloys alloyed with rhenium and ruthenium (review). Part 1. Aviation materials and technologies, 2023, no. 1 (70), paper no. 03. Available at: http://www.journal.viam.ru (accessed: December 04, 2023). DOI: 10.18577/2713-0193-2023-0-1-30-50.
- Gromov V.I., Yakusheva N.A., Vostrikov A.V., Cherkashneva N.N. High strength structural steels for gas-turbine engine shafts (review). Aviation materials and technology, 2021, no. 1 (62), paper no. 01. Available at: http://www.journal.viam.ru (accessed: December 04, 2023). DOI: 10.18577/2713-0193-2021-0-1-3-12.
- Kablov E.N., Chabina E.B., Morozov G.A., Muravskaya N.P. Assessing the conformity of new materials using high-level RM and MI. Kompetentnost, 2017, no. 2, pp. 40–46.
- State Standart 13151.11–77. Ferromolybdenum. Method for determining arsenic content. Moscow: Standards Publishing House, 1977, pp. 1–4.
- State Standart 13151.6–94. Ferromolybdenum. Phosphorus determination method. Moscow: Publishing house of standards, 1994, pp. 1–6.
- State Standart 13151.7–82. Ferromolybdenum. Methods for determining copper. Moscow: Publishing house of standards, 1982, pp. 3–4.
- Tsygankova A.R., Makashova G.V., Shelpakova I.R., Saprykin A.I. Analysis of molybdenum trioxide by ICP-AES. Analitika i kontrol, 2011, vol. 15, no. 2, pp. 182–186.
- Hu J., Wang H. Determination of Trace Elements in Super Alloy by ICP-MS. Mikrochimica Acta, 2001, vol. 137, pp. 149–155.
- Pupyshev A.A., Epova E.N. Spectral interference of polyatomic ions in the inductively coupled plasma mass spectrometry method. Analitika i kontrol, 2001, vol. 5, no. 4, pp. 335–369.
- Karandashev V.K., Turanov A.N., Nosenko S.V. Analysis of molybdenum oxide by atomic emission and inductively coupled plasma mass spectrometry. Zhurnal analiticheskoy khimii, 2011, vol. 66, no. 1, pp. 40–46.
- Jakubowski N., Prohaska T., Rottmann L., Vanhaecke F. Inductively coupled plasma- and glow discharge plasma-sector field mass spectrometry. Part I. Tutorial: Fundamentals and instrumentation. Journal of Analytical Atomic Spectrometry, 2011, vol. 26, pp. 693–726.
- Ganeev A.A., Gubal A.R., Uskov K.N., Potapov S.V. Analytical mass spectrometry with glow discharge. Izvestiya Akademii nauk. Seriya khimicheskaya, 2012, no. 4, pp. 1–15.