FSW-joints mechanical characteristics optimization by modern computing systems

Bakradze M.M., Panteleev M.D., Skupov A.A., Belozor V.E., Ponomarev P.A.
Bakradze M.M., Panteleev M.D., Skupov A.A., Belozor V.E., Ponomarev P.A. FSW-joints mechanical characteristics optimization by modern computing systems // Proceedings of VIAM. 2019. No. 4. DOI: 10.18577/2307-6046-2019-0-4-11-20. URL: https://www.viam-works.ru/en/journal/2019/4/2
Keywords
friction stir welding, regression model, aluminum-lithium alloys, mechanical properties, fatigue characteristics.
Abstract

The influence of the friction stir welding parameters of aluminum-lithium alloys V-1461 and V-1469 on welded joint surface roughness and mechanical properties has been investigated. Experiment planning was carried out and mathematical models for the dependencies of strength and roughness on the parameters of the FSW processwere developed. For each of the studied alloys a welding parameter range has been established, which ensures an increased purity of the weld surface after welding(Rz≤50 μm), absence of defects and the welded joint strength
level about 0,75–0,8 of the base metal strength.

Reference list
  1. Kablov E.N. Innovacionnye razrabotki FGUP «VIAM» GNC RF po realizacii «Strategicheskih napravlenij razvitiya materialov i tehnologij ih pererabotki na period do 2030 goda» [Innovative developments of FSUE «VIAM» SSC of RF on realization of «Strategic directions of the development of materials and technologies of their processing for the period until 2030»] // Aviacionnye materialy i tehnologii. 2015. №1 (34). S. 3–33. DOI: 10.18577/2071-9140-2015-0-1-3-33.
  2. Kablov E.N., Antipov V.V., Klochkova Yu.Yu. Alyuminiy-litiyevyye splavy novogo pokoleniya i sloistyye alyumostekloplastiki na ikh osnove [Aluminum-lithium alloys of a new generation and layered aluminum-glass plastics on their basis] // Tsvetnyye metally. 2016. №8 (884). S. 86–91. DOI: 10.17580/tsm.2016.08.13.
  3. Panteleev M.D., Bakradze M.M., Skupov A.A., Scherbakov A.V., Belozor V.E. Tekhnologicheskie osobennosti svarki plavleniem alyuminievogo splava V-1579 [Technological features of fusion welding of aluminum alloy V-1579] // Aviacionnye materialy i tehnologii. 2018. №3 (52). S. 11–17. DOI: 10.18577/2071-9140-2018-0-3-11-17.
  4. Antipov V.V., Serebrennikova N.Yu., Nefedova Yu.N., Kozlova O.Yu., Panteleev M.D., Osipov N.N., Klychеv A.V. Tekhnologicheskie osobennosti Izgotovleniya detalej iz alyuminiy-litievogo splava 1441 [Manufacturing capability of Al–Li 1441 alloy details] // Trudy VIAM: elektron. nauch.-tekhnich. zhurn. 2018. №10 (70). St. 03 Available at: http://www.viam-works.ru (accessed: Вусуьиук 03, 2018). DOI: 10.18577/2307-6046- 2018-0-10-17-26.
  5. Kablov E.N. Sovremennyye materialy – osnova innovatsionnoy modernizatsii Rossii [Modern materials - the basis of innovative modernization of Russia] // Metally Evrazii. 2012. №3. S. 10–15.
  6. Kablov E.N. Materialy dlya aviakosmicheskoy tekhniki [Materials for aerospace] // Vse materialy. Entsiklopedicheskiy spravochnik. 2007. №5. S. 7–27.
  7. Kablov E.N., Ospennikova O.G., Vershkov A.V. Redkie metally i redkozemelnye elementy – materialy sovremennyh i budushhih vysokih tehnologij [Rare metals and rare-earth elements are materials for modern and future high technologies] // Aviacionnye materialy i tehnologii. 2013. №S2. S. 3–10.
  8. Antipov V.V., Klochkova Yu.Yu., Romanenko V.A. Sovremennye alyuminievye i alyuminij-litievye splavy [Modern aluminum and aluminum-lithium alloys] // Aviacionnye materialy i tehnologii. 2017. №S. S. 195–211.
  9. Klochkova Yu.Yu., Grushko O.E., Lantsova L.P., Burlyaeva I.P., Ovsyannikov B.V. Osvoenie v promyshlennom proizvodstve polufabrikatov iz perspektivnogo alyuminijlitievogo splava V-1469 [Development in industrial production of semi-finished products from perspective aluminum lithium alloy V-1469] // Aviacionnye materialy i tehnologii. 2011. №1. S. 8–12.
  10. Shalin R.E., Eefremov I.S., Yarovinskiy Yu.L., Lukin V.I. Opyt proyektirovaniya i izgotovleniya krupnogabaritnykh konstruktsiy iz alyuminiyevo-litiyevykh splavov izdeliy raketno-kosmicheskoy tekhniki [Experience in the design and manufacture of large-sized structures of aluminum-lithium alloys products of rocket and space technology] //Svarochnoye proizvodstvo. 1996. №11. S. 14–18.
  11. Lukin V.I., Ioda Ye.N., Bazeskin A.V., Lavrenchuk V.P., Kotelnikova L.V., Oglodkov M.S. Povysheniye nadezhnosti svarnykh soyedineniy iz vysokoprochnogo alyuminiyevo-litiyevogo splava V-1461 []Improving the reliability of welded joints of high-strength aluminum-lithium alloy V-1461 // Svarochnoye proizvodstvo. 2010. №11. S. 14–17.
  12. Fomin V.M., Malikov A.G., Orishich A.M., Antipov V.V., Klochkov G.G., Skupov A.A. Vliyanie termicheskoj obrabotki na structure svarnykh soedinenij listov is splava V-1469 sistemy Al–Cu–Li, poluchennykh lazernij svarkoj [Heat treatment effect on structure of joint weld sheets from V-1469 alloy of Al–Cu–Li system manufactured by laser welding] // Aviacionnye materialy i tehnologii. 2018. №1 (50). S. 9–18. DOI: 10.18577/2071-9140-2018-0-1-9-18.
  13. Petrovic M., Veljic D., Rakin M. et al. Friction-stir welding of high-strength aluminium alloys and a numerical simulation of plunge stage // Materials in technology. 2012. Vol. 46. No. 3. P. 215–221.
  14. Sposob svarki metallov treniyem: avtorskoye svidetelstvo 195846 SSSR [Method of welding metals by friction: USSR author's certificate]; opubl. 04.05.67
  15. Mishra R.S., Ma Z.Y. Friction stir welding and processing // Journal Material Science Engineering. 2005. Vol. 50. P. 1–78.
  16. Shtrikman M.M. Sostoyaniye i razvitiye protsessa svarki treniyem lineynykh soyedineniy [The state and development of the process of friction welding of linear joints] // Svarochnoye proizvodstvo. 2007. №9. S. 35–40.
  17. Betsofen S.Ya., Sbitneva S.V., Panteleyev M.D., Bakradze M.M., Dolgova M.I., Kabanova Yu.V. Issledovaniye formirovaniya fazovogo sostava splava sistemy Al–Cu–Li V-1469 v protsesse svarki treniyem s peremeshivaniyem [Study of the formation of the phase composition of the Al – Cu – Li B-1469 system alloy during friction stir welding process] // Metally. 2018. №6. S. 54–63.
  18. Silis M.I., Eliseyev A.A., Silis V.E. i dr. Osobennosti struktury svarnykh soyedineniy alyuminiyevykh splavov, poluchennykh friktsionnoy svarkoy [Structural features of welded joints of aluminum alloys obtained by friction welding] // Metallovedeniye i termicheskaya obrabotka. 2009. №4. S. 34–39.
  19. Oglodkov M.S., Khokhlatova L.B., Kolobnev N.I., Alixeev A.A., Lukina E.A. Vliyanie termomekhanicheskoj obrabotki na svojstva i structuru splava sistemy Al–Cu–Mg–Li–Zn [Effect of the thermomecanical treatment on Al (Al–Cu–Mg–Li–Zn) alloy properties and structure] // Aviacionnye materialy i tehnologii. 2010. №4. S. 15–19.
  20. Yanfeng D., Zhijie T., Peitao G., Yanhua Z. Effect of process parameters on weld quality by friction stir welding of 2219 aluminum alloy // China Welding. 2011. Vol. 20. No. 2. P. 12–16.
  21. Lukin V.I., Samorukov M.L., Kovalchuk V.G. Modelirovaniye rotatsionnoy svarki treniyem vysokozharoprochnogo nikelevogo splava VZh175 [Simulation of rotational friction welding of high-temperature nickel alloy VZh175] // Svarochnoye proizvodstvo. 2016. №11. S. 12–18.
  22. Samorukov M.L. Analiticheskij podhod k matematicheskomu modelirovaniyu temperaturnoj sostavlyayushhej rotacionnoj svarki treniem [Analytical approach to mathematical modeling of temperature component of direct drive friction welding] // Trudy VIAM: elektron. nauch.-tehnich. zhurn. 2013. №9. St. 03. Available at: http://www.viam-works.ru (accessed: October 31, 2018).
  23. Dolzhanskiy Yu.M., Novik F.S., Chemleva T.A. Planirovaniye eksperimenta pri issledovanii i optimizatsii svoystv splavov: metodich. posobiye [Planning an experiment in the study and optimization of properties of alloys: Toolkit]. M.: VIAM, 1974. 132 s.
  24. Lukin V.I., Ioda E.N., Skupov A.A., Panteleev M.D., Ovchinnikov V.V., Malov D.V. Effect of the surface roughness of friction stir welded joints on the fatigue characteristics of welded joints in V-1461 and V-1469 aluminium-lithium alloys // Welding International. 2017. Vol. 31:12. P. 974–978. DOI: 10.1080/09507116.2017.1369062.
  25. Kheyvud R.B. Proyektirovaniye s uchetom ustalosti [Design taking into account fatigue]. M.: Mashinostroyeniye, 1969. 503 s.