Microstructure and properties investigations of Fe–Cr–Ni stainless steel obtained by selective laser melting
Bogachev I.A., Sulyanova E.A., Sukhov D.I., Mazalov P.B. Microstructure and properties investigations of Fe–Cr–Ni stainless steel obtained by selective laser melting // Proceedings of VIAM. 2019. No. 3. DOI: 10.18577/2307-6046-2019-0-3-3-13. URL: https://www.viam-works.ru/en/journal/2019/3/1
Keywords
stainless steel, microstructure, mechanical properties anisotropy, selective laser melting, heat treatment, recrystallization.
Abstract
Microstructure investigations of Fe–Cr–Ni stainless steel’s sintered samples obtained by selective laser melting were held. Mechanical properties and corrosion resistance of the samples at the initial state and after treatment were estimate. It is shown that material’s structure consists of fine grain sells oriented along the crystallization direction. After hot isostatic pressing and heat treatment microstructure becomes more homogeneous and takes the form of identical one of the casting material. Anisotropy of the mechanical properties intrinsic to the sintered state is not observed.
Reference list
- Kablov E.N. Nastoyashcheye i budushcheye additivnykh tekhnologiy [Present and future of additive technologies] // Metally Evrazii. 2017. №1. S. 2–6.
- Kablov E.N. Additivnyye tekhnologii – dominanta natsional'noy tekhnologicheskoy initsiativy [Additive technologies – the dominant of the national technology initiative] // Intellekt i tekhnologii. 2015. №2 (11). S. 52–55.
- Gromov V.I., Voznesenskaya N.M., Pokrovskaya N.G., Tonysheva O.A. Vysokoprochnye konstrukcionnye i korrozionnostojkie stali FGUP «VIAM» dlya izdelij aviacionnoj tehniki [High-strength constructional and corrosion-resistant steels developed by VIAM for aviation engineering] // Aviacionnye materialy i tehnologii. 2017. №S. S. 159–174. DOI: 10.18577/2071-9140-2017-0-S-159-174.
- Voznesenskaya N.M., Kablov E.N., Petrakov A.F., Shalkevich A.B. Vysokoprochnyye korrozionnostoykiye stali austenitno-martensitnogo klassa [High-strength corrosion-resistant steels of austenitic-martensitic class] // Metallovedeniye i termicheskaya obrabotka metallov. 2002. №7. S. 34–37.
- Markova E.S., Pokrovskaya N.G., Shalkevich A.B., Gromov V.I. Martensitostareyushhie stali ‒ novye perspektivnye materialy dlya valov GTD [Maraging became ‒ new perspective materials for GTE shaft] // Aviacionnye materialy i tehnologii. 2012. №S. S. 81–84.
- Kablov E.N. Innovacionnye razrabotki FGUP «VIAM» GNC RF po realizacii «Strategicheskih napravlenij razvitiya materialov i tehnologij ih pererabotki na period do 2030 goda» [Innovative developments of FSUE «VIAM» SSC of RF on realization of «Strategic directions of the development of materials and technologies of their processing for the period until 2030»] // Aviacionnye materialy i tehnologii. 2015. №1 (34). S. 3–33. DOI: 10.18577/2071-9140-2015-0-1-3-33.
- Li R., Shi Y., Wang Z. et al. Densification behavior of gas and water atomized 316L stainless steel powder during selective laser melting // Applied Surface Science. 2010. Vol. 256. No. 13. P. 4350–4356.
- Li R., Liu J., Shi Y. et al. 316L Stainless Steel with Gradient Porosity Fabricated by Selective Laser Melting // Journal of Materials Engineering and Performance. 2009. Vol. 19. No. 5. P. 667–671.
- Kempen K., Yasa E., Thijs L. et al. Microstructure and mechanical properties of Selective Laser Melted 18Ni-300 steel // Physics Procedia. 2011. Vol. 12. P. 255–263.
- Tonysheva O.A., Voznesenskaya N.M., Shestakov I.I., Eliseyev E.A. Vliyaniye rezhimov vysokotemperaturnoy termomekhanicheskoy obrabotki na strukturu i svoystva vysokoprochnoy korrozionnostoykoy stali austenito-martensitnogo klassa 17KH13N4K6SAM3ch [Influence of modes of high-temperature thermomechanical processing on structure and properties of high-strength corrosion-resistant steel of austenitic-martensitic class 17Х13Н4К6САМ3ч] // Aviacionnyye materialy i tehnologii. 2017. №1 (46). S. 11–16. DOI: 10.18577/2307-6046-2017-0-1-11-16.
- Kablov E.N., Krivonogov G.S. Legirovaniye i fazovaya nestabilnost vysokoprochnykh korrozionnostoykikh staley [Doping and phase instability of high-strength corrosion-resistant steels] // Metally. 2002. №2. S. 65–73.
- Tonysheva O.A., Voznesenskaya N.M. Perspektivnye vysokoprochnye korrozionnostojkie stali, legirovannye azotom (sravnitelnyj analiz) [Perspective high-strength corrosion-resistant steels alloyed with nitrogen (comparative analysis] // Aviacionnye materialy i tehnologii. 2014. №3. S. 27–32.
- Rafi H.K., Starr T.L., Stucker B.E. A comparison of the tensile, fatigue, and fracture behavior of Ti–6Al–4V and 15-5 PH stainless steel parts made by selective laser melting // International Journal of Advanced Manufacturing Technology. 2013. Vol. 69. No. 5–8. P. 1299–1309.
- Guan K., Wang Z., Gao M. et al. Effects of processing parameters on tensile properties of selective laser melted 304 stainless steel // Materials and Design. 2013. Vol. 50. P. 581–586.
- Karpov D., Em V.T., Mazalov P.B., Sulyanova E.A. Characterization of residual stresses by neutron diffraction at the research reactor IR-8 of NRC «Kurchatov Institute» // Journal of Physics: Conference Series. 2018. DOI:10.1088/1742-6596/1109/1/012046.
- Kablov E.N., Nikiforov A.A., Demin S.A., Chesnokov D.V., Vinogradov S.S. Perspektivnyye pokrytiya dlya zashchity ot korrozii uglerodistykh staley [Perspective coatings for corrosion protection of carbon steels] // Stal. 2016. №6. S. 70–81.