Regular features of silicon behavior in melting and directional solidification of single-crystal superalloys

Min P.G., Sidorov V.V., Vadeev V.E.
Min P.G., Sidorov V.V., Vadeev V.E. Regular features of silicon behavior in melting and directional solidification of single-crystal superalloys // Proceedings of VIAM. 2017. No. 4. DOI: 10.18577/2307-6046-2017-0-4-3-3. URL: https://www.viam-works.ru/en/journal/2017/4/3
Keywords
silicon, ceramic, mold, superalloy, impurities, directional solidification, refinement.
Abstract

The silicon reduction from a ceramic mold on account of melt interaction in directional solidification of ZhS32-VI and VZhM5-VI single-crystal superalloys for gas turbine blades was studied. It is proved that saturation with silicon took place for a reason of interaction of carbon with free silicon oxide included in the composition of the ceramic mold. It is founded that saturation with silicon occurs of non-carbon single-crystal alloys 4 times slower than carbon-containing alloys. The possibility of form refractory compounds with sulfur and yttrium which remove from melt by filtration with different speed was confirmed. But low efficiency of this method waw founded.

Reference list
  1. Sidorov V.V., Rigin V.E., Timofeeva O.B., Min P.G. Vliyanie kremniya i fosfora na zharoprochnye svojstva i strukturno-fazovye prevrashheniya v monokristallah iz vysokozharoprochnogo splava VZhM4-VI [An effect of silicon and phosphorus on high temperature properties and structure-phase transformations of single crystals of VGM4-VI superalloy] // Aviacionnye materialy i tehnologii. 2013. №3. S. 32–38.
  2. Tigrova G.D., Korkka S.I., Grebcova T.M. Vliyanie kremniya na fazovyj sostav splavov na nikelevoj osnove [Influence of silicon on phase composition of nickel-based alloys] // MiTOM. 1980. №4. S. 38–41.
  3. Sidorov V.V., Morozova G.I., Petrushin N.V. i dr. Fazovyj sostav i termostabilnost litejnogo zharoprochnogo nikelevogo splava s kremniem [Phase structure and thermostability of cast heat resisting nickel alloy with silicon] // Metally. 1990. №1. S. 94–98.
  4. Sidorov V.V., Rigin V.E., Min P.G., Folomejkin Yu.I., Timofeeva O.B., Filonova E.V., Ishodzhanova I.V. Vliyanie primesej na strukturu i svojstva vysokozharoprochnyh litejnyh splavov i razrabotka effektivnyh metodov ustraneniya ih otricatelnogo vliyaniya [Influence of impurity on structure and property of high-heat resisting cast alloys and development of effective methods of elimination of their negative influence] // Novosti materialovedeniya. Nauka i tehnika: elektron. nauch.-tehnich. zhurn. 2014. №2. St. 03. Available at: http://www.materialsnews.ru (accessed: March 07, 2017).
  5. Sidorov V.V., Rigin V.E., Min P.G., Folomejkin Yu.I. Vliyanie fosfora i kremniya na strukturu i svojstva vysokozharoprochnyh litejnyh splavov i razrabotka effektivnyh metodov ustraneniya ih otricatelnogo vliyaniya [Influence of phosphorus and silicon on structure and properties of high-heat resisting cast alloys and development of effective methods of elimination of their negative influence] // MiTOM. 2015. №6 (720). S. 55–59.
  6. Sidorov V.V., Rigin V.E., Min P.G., Folomeikin Yu.I. Effect of phosphorus and silicon on structure and properties of highly refractory cast alloys and development of effective methods for eliminating their unfavorable effect // Metal Science and Heat Treatment. 2015. Vol. 57. No. 5–6. P. 364–368.
  7. Sidorov V.V., Min P.G., Burcev V.T., Kablov D.E., Vadeev V.E. Komp'yuternoe modelirovanie i eksperimentalnoe issledovanie reakcij rafinirovaniya v vakuume slozhnolegirovannyh renijsoderzhashhih nikelevyh rasplavov ot primesej sery i kremniya [Computer modeling and pilot study of reactions of refinement in vacuum complex-alloyed rhenium containing nickel melt from sulfur and silicon impurity] // Vestnik RFFI. 2015. №1 (85). S. 32–36.
  8. Sidorov V.V., Min P.G. Rafinirovanie slozhnolegirovannogo nikelevogo rasplava ot primesi sery pri plavke v vakuumnoj indukcionnoj pechi. Chast 1 [Refinement complex-alloyed nickel melt from sulfur impurity when melting in the vacuum induction furnace. Part 1] // Elektrometallurgiya. 2014. №3. S. 18–23.
  9. Sidorov V.V., Min P.G. Rafinirovanie slozhnolegirovannogo nikelevogo rasplava ot primesi sery pri plavke v vakuumnoj indukcionnoj pechi. Chast 2 [Refinement complex-alloyed nickel melt from sulfur impurity when melting in the vacuum induction furnace. Part 2] // Elektrometallurgiya. 2014. №5. S. 26–30.
  10. Sidorov V.V., Min P.G., Folomejkin Yu.I., Vadeev V.E. Vliyanie skorosti filtracii slozhnolegirovannogo nikelevogo rasplava cherez penokeramicheskij filtr na soderzhanie primesi sery v metalle [Influence of speed of filtering complex-alloyed nickel melt via the foamceramic filter on the content of impurity of sulfur in metal] // Elektrometallurgiya. 2015. №5. S. 12–15.
  11. Sidorov V.V., Rigin V.E., Min P.G., Folomejkin Yu.I. Issledovanie processov rafinirovaniya v vakuume slozhnolegirovannyh nikelevyh rasplavov ot primesi sery [Research of refining processes in vacuum complex-alloyed nickel melt from sulfur impurity] // Metally. 2015. №6. S. 57–63.
  12. Min P.G., Sidorov V.V., Kablov D.E., Rigin V.E., Vadeev V.E. Issledovanie sery i fosfora v litejnyh zharoprochnyh nikelevyh splavah i razrabotka effektivnyh sposobov ih rafinirovaniya [Sulfur and phosphorus research in cast heat resisting nickel alloys and development of effective ways of their refinement] // Tehnologiya metallov. 2015. №12. S. 2–9.
  13. Min P.G., Sidorov V.V. Opyt pererabotki litejnyh othodov splava ZhS32-VI na nauchno-proizvodstvennom komplekse VIAM po izgotovleniyu lityh prutkovyh (shihtovyh) zagotovok [The experience of GS32-VI alloy scrap recycling at the VIAM scientific and production complex for cast bars production] // Aviacionnye materialy i tehnologii. 2013. №4. S. 20–25.
  14. Kablov E.N., Ospennikova O.G., Sidorov V.V., Rigin V.E., Kablov D.E. Osobennosti tehnologii vyplavki sovremennyh litejnyh vysokozharoprochnyh nikelevyh splavov [Features of smelting technology of modern cast high-heat resisting nickel alloys] // Vestnik MGTU im. N.E. Baumana. Ser.: Mashinostroenie. 2011. №SP. C. 68–78.
  15. Sidorov V.V., Rigin V.E., Goryunov A.V., Min P.G., Kablov D.E. Poluchenie Re–Ru soderzhashhego splava s ispolzovaniem nekondicionnyh othodov [Receiving Re–Ru of containing alloy with use of unconditioned waste] // Metallurgiya mashinostroeniya. 2012. №3. S.15–17.
  16. Sidorov V.V., Rigin V.E., Goryunov A.V., Min P.G. Resursosberegayushhaya tehnologiya pererabotki nekondicionnyh othodov litejnyh zharoprochnyh splavov [Resource-saving refining technology of unconditioned waste of foundry hot strength alloys] // Metallurg. №5. 2014. S. 35–39.
  17. Kablov E.N., Sidorov V.V., Kablov D.E., Rigin V.E., Goryunov A.V. Sovremennye tehnologii polucheniya prutkovyh zagotovok iz litejnyh zharoprochnyh splavov novogo pokoleniya [Modern technologies of receiving the bar stock preparations from foundry heat resisting alloys of new generation] // Aviacionnye materialy i tehnologii. 2012. №S. S. 97–105.
  18. Sidorov V.V., Rigin V.E., Goryunov A.V., Min P.G. Opyt pererabotki v usloviyah FGUP «VIAM» litejnyh othodov zharoprochnyh splavov, obrazuyushhihsya na motorostroitelnyh i remontnyh zavodah [Experience of processing in the conditions of FSUE «VIAM» of foundry waste of the hot strength alloys which are forming at engine-building and repair plants] // Metallurg. 2014. №1. S. 86–90.
  19. Sidorov V.V., Rigin V.E., Gorjunov A.V., Min P.G. Innovatsionnaya tehnologiya proizvodstva zharoprochnogo splava ZhS32-VI s uchetom pererabotki vseh vidov othodov v usloviyah sertificirovannogo serijnogo proizvodstva FGUP «VIAM» [The innovation technology of high temperature GS32-VI alloy production considering the recycling of all scrap appearance a certificated quantity production of FGUP «VIAM»] // Trudy VIAM: elektron. nauch.-tehnich. zhurn. 2014. №6. St. 01. Available at: http://www.viam-works.ru (accessed: March 07, 2017). DOI: 10.18577/2307-6046-2014-0-6-1-1.
  20. Min P.G., Goryunov A.V., Vadeev V.E. Sovremennye zharoprochnye nikelevye splavy i effektivnye resursosberegayushhie tehnologii ih izgotovleniya [Modern heat resisting nickel alloys and effective resource-saving technologies of their manufacturing] // Tehnologiya metallov. 2014. №8. S. 12–23.
  21. Kablov E.N., Sidorov V.V., Kablov D.E., Min P.G., Rigin V.E. Resursosberegayushhie tehnologii vyplavki perspektivnyh litejnyh i deformiruemyh superzharoprochnyh splavov s uchetom pererabotki vseh vidov othodov [Resource-saving smelting technologies of perspective cast and deformable superhot strength alloys taking into account processing of all types of waste] // Elektrometallurgiya. 2016. №9. S. 30–41.
  22. Sidorov V.V., Rigin V.E., Goryunov A.V., Min P.G. Processing Superalloy Foundry Waste Generated at Engine Building and Repair Plants: Experience of the All-Russia Research Institute of Aviation Materials // Metallurgist. 2014. Vol. 58. No. 1–2. P. 69–74.
  23. Sidorov V.V., Rigin V.E., Goryunov A.V., Min P.G. Resources-saving technology for recycling off-grade waste products cast from superalloys // Metallurgist. 2014. Vol. 58. No. 5–6. P. 360–366.
  24. Min P.G., Goryunov A.V., Vadeev V.E. Modern Nickel Superalloys and the Efficient Resource-Saving Technologies of Their Production // Russian Metallurgy (Metally). 2015. No. 13. P. 1060–1068.
  25. Kablov E.N., Sidorov V.V., Kablov D.E., Min P.G., Rigin V.E. Resource-Saving Technologies of Making Advanced Cast and Deformable Superalloys with Allowance for Processing All Types of Wastes // Russian Metallurgy (Metally). 2016. No. 12. P. 1187–1195.
  26. Ospennikova O.G., Min P.G., Vadeev V.E., Kalitsev V.A., Kramer V.V. Resursosberegayushhaya tehnologiya pererabotki nekondicionnyh othodov deformiruemogo splava VZh175 dlya diskov GTD [Resource-saving processing technology of off-grade scrap of wrought superalloy VG175 for GTE disks production] // Trudy VIAM: elektron. nauch.-tehnich. zhurn. 2016. №2. St. 01. Available at: http://www.viam-works.ru (accessed: March 07, 2017). DOI: 10.18577/2307-6046-2016-0-2-1-1.
  27. Kablov E.N. Innovacionnye razrabotki FGUP «VIAM» GNC RF po realizacii «Strategicheskih napravlenij razvitiya materialov i tehnologij ih pererabotki na period do 2030 goda» [Innovative developments of FSUE «VIAM» SSC of RF on realization of «Strategic directions of the development of materials and technologies of their processing for the period until 2030»] // Aviacionnye materialy i tehnologii. 2015. №1 (34). S. 3–33. DOI: 10.18577/2071-9140-2015-0-1-3-33.
  28. Yakimovich P.V., Alekseev A.V., Min P.G. Opredelenie nizkih soderzhanij fosfora v zharoprochnyh nikelevyh splavah metodom ISP-MS [Determination of low phosphorus content in heat-resistant nickel alloys by ICP-MS method] // Trudy VIAM : elektron. nauch.-tehnich. zhurn. 2014. №10. St. 02. Available at: http://viam-works.ru (accessed: March 07, 2017). DOI: 10.18577/2307-6046-2014-0-10-2-2.
  29. Mehanik E.A., Min P.G., Gundobin N.V., Rastegaeva G.Yu. Opredelenie massovoj doli sery v zharoprochnyh nikelevyh splavah i stalyah v diapazone koncentracij ot 0,0001 do 0,0009% (po masse) [Determination of sulfur mass fraction in heat-resistant nickel alloy and steels within the concentration range from 0,0001 to 0,0009% wt.] // Trudy VIAM : elektron. nauch.-tehnich. zhurn. 2014. №9. St. 12. Available at: http://viam-works.ru (accessed: March 07, 2017). DOI: 10.18577/2307-6046-2014-0-9-12-12.
  30. Lyakishev N.P., Alisova S.P., Bannyh O.A. i dr. Diagrammy sostoyaniya dvojnyh metallicheskih sistem: spravochnik [Charts of condition of double metal systems: directory]. M.: Mashinostroenie, 2000. T. III, kn. 1. 837 s.