N. V. Antyufeeva, I. V. Zelenina, A. V. Nacharkina, A. V. Kosyakova, A. V. Efremova, P. S. Marakhovsky Effect of heat treatment on the strength and thermophysical characteristics of polyimide carbon fiber reinforced plastic // Proceedings of VIAM. 2026. No. 11 (165). С. 165-179. URL: https://www.viam-works.ru. DOI: 10.18577/2307-6046-2026-0-11-165-179.

Effect of heat treatment on the strength and thermophysical characteristics of polyimide carbon fiber reinforced plastic

N. V. Antyufeeva1, I. V. Zelenina1, A. V. Nacharkina1, A. V. Kosyakova1, A. V. Efremova1, P. S. Marakhovsky1

1Federal State Unitary Enterprise «All-Russian Scientific-Research Institute of Aviation Materials» of National Research Center «Kurchatov Institute», Moscow, Russia; admin@viam.ru

Abstract

In the study was investigated the effect of additional heat treatment at temperatures of 300, 320, and 350 °C on the properties of polyimide-based carbon fiber reinforced plastic. It was shown that increasing the post-curing temperature raises the glass transition temperature from 336 to 358 °C. When tested under room temperature conditions and after heat treatment, the flexural strength and interlaminar shear strength of the material decreased. Furthermore, the heat treatment influenced the thermophysical properties: coefficient of linear thermal expansion, thermal conductivity, thermal diffusivity and specific heat capacity.

Keywords
carbon fiber reinforced plastic, heat treatment, polyimide binder, high-temperature composite materials, strength characteristics, thermophysical properties


Reference list
  1. Mukhametov R.R., Petrova A.P. Thermosetting Binders for Polymer Composite Materials: Textbook. Ed. E.N. Kablov. Moscow: NRC «Kurchatov Institute» – VIAM, 2021, 528 p.
  2. Kablov E.N., Startsev V.O. Systematical analysis of the climatics influence on mechanical properties of the polymer composite materials based on domestic and foreign sources (review). Aviacionnye materialy i tehnologii, 2018, no. 2 (51), pp. 47–58. DOI: 10.18577/2071-9140-2018-0-2-47-58.
  3. Xiaochen L., Bo C.J., Thomas K.T., Steven N. Thermo-oxidative aging and thermal cycling of PETI-340M composites. High Performance Polymers, 2022, vol. 34, pp. 33–43.
  4. Bain S., Ozawa S., Jim M., Criss Jr. Development of a Cure/Postcure Cycle for PETI-330 Laminates Fabricated by Resin Transfer Molding. High Performance Polymers, 2006. Available at: https://www.academia.edu/5559484/Development of a Cure Postcure Cycle for PETI-330 Laminates Fabricated by Resin Transfer Molding (accessed: April 10, 2026).
  5. Fernberg P., Gong G., Mannberg P., Tsampas S. Development of novel high Tg polyimide-based composites. Part I: RTM processing properties. Journal of Composite Materials, 2018, vol. 52, no. 2, pp. 253–260.
  6. Gao S.Z., Huang Z.Q., Wang X.L. et al. Research on Properties of 450 °С Resistant Polyimide Composites. Journal of Physics: Conference Series (ISALT 2022), 2023, vol. 2460, no. 012091, pp. 1–8. DOI: 10.1088/1742-6596/2460/1/012091.
  7. Mikhailin Yu.A. Heat-Resistant Polymers and Polymeric Materials. St. Petersburg: Professiya, 2006, 624 p.
  8. Kerber M.L., Vinogradov V.M., Golovkin G.S. et al. Polymer Composite Materials: Structure, Properties, Technology: Textbook. Ed. A.A. Berlin. St. Petersburg: Professiya, 2008, 560 p.
  9. Valueva M.I., Zelenina I.V., Nacharkina A.V., Ahmadieva K.R. Technological features of obtaining high temperature polyimide carbons. Foreign experience (review). Trudy VIAM, 2022, no. 6 (112), pp. 80–95. Available at: http://www.viam-works.ru (accessed: April 10, 2026). DOI: 10.18577/2307-6046-2022-0-6-80-95.
  10. CYCOM®5250 Bismaleimide Resin. Technical Data Sheet. Cytec engineered materials. 2017. Available at: https://www.solvay.com/en/product/cycom-5250-4 (accessed: April 03, 2026).
  11. Nacharkina A.V., Valueva M.I., Zelenina I.V., Shosheva A.L. High-temperature carbon fiber reinforced plastics based on bismaleinimide binders. Aviation materials and technologies, 2024, no. 4 (77), pp. 43–61. Available at: http://www.journal.viam.ru (accessed: April 10, 2026). DOI: 10.18577/2713-0193-2024-0-4-43-61.
  12. Mikhailin Yu.A. Heat, Thermal, and Fire Resistance of Polymer Materials. St. Petersburg: Nauchnyye osnovy i tekhnologii, 2011, 416 p.
  13. Strelnikov V.N., Ivanova E.V., Lebedeva Е.А., Trukhinov D.K., Astafeva S.А. Development and research of the properties of thermoplastic elastomer composites with functional fillers. Aviation materials and technologies, 2026, no. 1 (82), pp. 195–208. Available at: http://www.journal.viam.ru (accessed: April 28, 2026). DOI: 10.18577/2713-0193-2026-0-1-195-208.
  14. Gulyaev I.N., Klimenko O.N., Lonskii S.L., Slavin A.V., Cherfas L.V. Determination of the composition and structure of polymer composite materials. Aviation materials and technologies, 2025, no. 4 (81), pp. 32–47. Available at: http://www.journal.viam.ru (accessed: April 14, 2026). DOI: 10.18577/2713-0193-2025-0-4-32-47.
  15. Valueva M.I., Zelenina I.V., Zharinov M.A., Khaskov M.A. High-Temperature Carbon Fiber Reinforced Plastics Based on a Thermoreactive Polyimide Binder. Inorganic Materials: Applied Research, 2021, vol. 12, no. 6, pp. 1581–1589.
  16. Adamczak A.D. High temperature materials for aerospace applications. Texas A&M University, 2011, 139 p.
  17. Choy C.L., Luk W.H., Chen F.C. Thermal conductivity of highly oriented polyethylene. Polymer, 1978, vol. 19, pp. 155–162.
  18. Fei H., Dai W., Yu J. et al. Thermal diffusivity and thermal conductivity of polyimide composites. Journal of Applied Polymer Science, 2019, vol. 136, no. 15, p. 47336.
  19. Pielichowska K. Polyimide-based composites for high-temperature applications. Progress in Materials Science, 2014, vol. 67, pp. 173–232.
  20. Xiong X., Yang S.Y., Ji M. et al. Thermal expansion behavior of polyimide composites. Polymer Composites, 2018, vol. 39, no. S3, pp. E1688–E1695.